A chelated lithium molybdenum ion lubricating oil additive and its preparation method and application
By alkylating and aminating kaolin and combining it with chelated lithium molybdenum ions to form a chelated lithium molybdenum ion lubricating oil additive, the problem of poor dispersion stability of kaolin in lubricating oil is solved and better friction reduction is achieved. Anti-wear effect and lubrication efficiency.
Patent Information
- Application Number
- CN202310362382.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-04-07
AI Technical Summary
The solid granularity and chemical activity of kaolin in existing lubricating oils lead to poor dispersion stability in liquid lubricating media, making it difficult to exert friction-reducing, anti-wear and self-healing functions, and easily causing abrasive wear.
By alkylating and aminating kaolin, and combining it with chelated lithium molybdenum ions, a chelated lithium molybdenum ion lubricating oil additive is formed, which improves its dispersion and solubility in oil and enhances friction reduction and anti-wear capabilities.
It improves the dispersion of lubricating oil and the repair ability of the friction pair surface, reduces the fluid resistance and viscosity, and enhances the lubrication efficiency and anti-friction ability.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lubricating oils, and in particular to a chelated lithium-molybdenum ion lubricating oil additive and a preparation method and application thereof. Background Art
[0002] Lubricating oil is a liquid or semi-solid lubricating oil used in mechanical parts of aviation, mechanical processing, metallurgy, automobile, transportation, coal and other industries to reduce friction and protect machinery and processed parts. It mainly plays the role of lubrication, auxiliary cooling, rust prevention, cleaning, sealing and buffering. Lubricating oil is generally composed of two parts: base oil and additives. Base oil is the main component of lubricating oil and determines the basic properties of lubricating oil. Additives make up for and improve the deficiencies in the performance of base oil and give lubricating oil some new properties. They are an important part of lubricating oil. Its type, quality and addition ratio directly affect the performance of lubricating oil.
[0003] Nano-additives are mainly used as friction reducers, anti-wear agents, extreme pressure agents, running-in agents, etc. in lubrication. Their special effects (such as surface interface effect, small size effect, volume effect, etc.) enable them to acquire new physical and chemical properties, and have excellent performance that traditional additives or lubricants cannot match. Therefore, they have the prospect of replacing traditional additives.
[0004] With people's increasing attention to environmental protection and the continuous development of nanomaterial technology, the development of green, pollution-free / low-pollution micro-nano lubricant additives has become a rapidly developing research direction. Two-dimensional layered materials have a lamellar structure, that is, the atoms in each atomic layer are bound together by strong covalent bonds, and the adjacent atomic layers are bound together by weak van der Waals forces. The layers are easy to slide, and the materials widely used for solid lubrication all have a lamellar structure. The silicate minerals in the two-dimensional layered materials are pollution-free to the environment and low in price. Studies have shown that silicate minerals, such as kaolin, montmorillonite, serpentine, etc., have certain friction reduction and anti-wear effects as lubricant additives.
[0005] Chinese patent document CN107446682A discloses a high-performance water-soluble lubricant for a rack, comprising the following components in parts by weight: 80-100 parts of base oil, 3-5 parts of hydroxyethyl cellulose, 6-8 parts of sodium polyacrylate, 8-12 parts of ethylene glycol, 1-2 parts of modified graphite powder, 3-9 parts of a blend of nano-kaolin and nano-alumina, 0.3-0.5 parts of polyvinyl alcohol emulsion, 5-15 parts of a stabilizer, 2-10 parts of a surfactant, 0.2-1 parts of a defoamer, and 30-70 parts of deionized water; the various additives are compounded to improve the various properties of the lubricant, increase the stability and lubricating effect of the lubricant, and effectively prevent the tooth surface of the rack from being damaged by wear, abrasion, and the like, thereby extending the service life of the rack.
[0006] However, the solid particle nature, high chemical activity, and easy adsorption of kaolin itself lead to its poor dispersion stability in liquid lubrication media, and it is easy to produce agglomeration and precipitation. Not only can it not play a good role in reducing friction and anti-wear self-repairing functions, but it may also cause abrasive wear due to agglomeration.
[0007] Ionic liquids are ideal lubricating materials because of their non-volatility, non-flammability, thermal stability, low melting point, and good electrical conductivity. In 2001, Ye et al. first discovered that ionic liquids are a type of multi-purpose lubricant with excellent performance. They conducted in-depth and systematic research on ionic liquid lubricating materials, which attracted widespread attention from researchers at home and abroad. So far, ionic liquids have been widely used as base oils, additives, lubricating films, and conductive greases. Studies have found that ordinary ionic liquids are soluble in polyethylene glycol with a higher polarity, but their solubility in hydrocarbon lubricants with a lower polarity is very low (<<1%). Summary of the invention
[0008] In order to solve the deficiencies in the prior art, the purpose of the present invention is to provide a chelated lithium molybdenum ion lubricating oil additive and a preparation method and application thereof. The prepared additive has good dispersibility in base oil and has good friction reduction and anti-wear effects.
[0009] In order to achieve the above object, the present invention adopts the following technical solution:
[0010] A method for preparing a chelated lithium molybdenum ion lubricating oil additive comprises the following steps:
[0011] (1) adding kaolin and hexadecyltrimethoxysilane into deionized water, magnetically stirring, ultrasonically treating, and then stirring to react. After the reaction is completed, filtering, washing, and drying the reaction product to obtain alkylated kaolin;
[0012] (2) adding alkylated kaolin and aminopropyltrimethoxysilane into deionized water, magnetically stirring, ultrasonically treating, and then stirring to react. After the reaction is completed, centrifuging, washing, and drying the reaction product to obtain amino / alkylated kaolin;
[0013] (3) Adding amino / alkylated kaolin to the chelated lithium molybdenum ion solution, stirring for reaction, and after the reaction is completed, filtering, washing, and drying the reaction product to obtain a chelated lithium molybdenum ion lubricant additive.
[0014] Preferably, in step (1), the mass volume ratio of kaolin, hexadecyltrimethoxysilane and deionized water is 1 g: 0.05-0.5 g: 100 mL.
[0015] Preferably, in step (1), magnetic stirring is performed for 10 to 20 minutes, and ultrasonic treatment is performed for 30 to 60 minutes; and the reaction conditions are 40 to 60° C. and the reaction is performed for 2 to 6 hours.
[0016] Preferably, in step (2), the mass volume ratio of alkylated kaolin, aminopropyltrimethoxysilane and deionized water is 1 g: 0.05-0.2 g: 100 mL.
[0017] Preferably, in step (2), the magnetic stirring time is 15 to 30 min, and the ultrasonic treatment time is 10 to 20 min; the reaction conditions are 50 to 80° C. and the reaction time is 4 to 10 h.
[0018] Preferably, in step (3), the chemical formula of the chelated lithium molybdenum ion is Li 2 C 10 H 16 N 2 O 8 Mo, the concentration of chelated lithium molybdenum ion solution is 0.1~1wt%.
[0019] Preferably, in step (3), the preparation method of the chelated lithium molybdenum ion solution is as follows: weigh EDTA and dissolve it in dilute ammonia water to form an EDTA solution with a concentration of 1 mol / L; weigh lithium acetate and molybdenum nitrate at a molar ratio of EDTA: Li: Mo of 1: 1~2: 0.5~1, add them to the EDTA solution, and stir the reaction at 80°C for 2h to obtain a chelated lithium molybdenum ion solution.
[0020] Preferably, in step (3), the reaction conditions are stirring the reaction at 70-90° C. for 6-10 hours; and the mass volume ratio of amino / alkylated kaolin to chelated lithium molybdenum ion solution is 1 g: 30-50 mL.
[0021] The present invention also claims to protect a lubricating oil additive prepared by the method.
[0022] The present invention also claims a use of the additive in lubricating oil, wherein the concentration of the additive in the lubricating oil is 0.01-0.13wt%;
[0023] Preferably, the lubricating oil includes Kunlun Scorpio F5000 lubricating oil, SF15W-40 lubricating oil and Great Wall SJ10W-40 lubricating oil, or mineral base oil and synthetic base oil.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1) The chelated lithium-molybdenum particle lubricating oil additive provided by the present invention has a layered structure of kaolin that is beneficial to reducing momentum transfer between fluid layers and separating the fluid layers, thereby reducing fluid resistance and lowering oil viscosity; kaolin is modified successively with hexadecyltrimethoxysilane and aminopropyltrimethoxysilane, which increases the dispersibility of kaolin in oil products, can bring more lubricating oil molecules to the surface of the friction pair, and form a layer of mechanical deposition film in the pits of the friction pair, which plays a filling and repairing role, thereby improving lubrication efficiency.
[0026] 2) The chelated lithium molybdenum particle lubricating oil additive provided by the present invention grafts the chelated lithium molybdenum ions onto the surface of amino / alkylated kaolin, thereby increasing the compatibility of the chelated lithium molybdenum ions with the oil phase. During the friction process, the chelated lithium molybdenum ions can undergo complex tribochemical reactions with the surface elements of the friction pair, generating a boundary lubrication film on the surface of the friction pair, thereby enabling the additive to have good friction reduction and anti-friction capabilities. Implementation
[0027] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0028] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.
[0029] Kaolin was purchased from Fuhua Nanomaterials Company, with a particle size of 0.5-2 μm;
[0030] The chelated lithium molybdenum ion solution was provided by Asia Sky Group.
[0031] The present invention will be further described below through specific embodiments. Example
[0032] A method for preparing a chelated lithium molybdenum ion lubricating oil additive comprises the following steps:
[0033] (1) 1 g of kaolin and 0.5 g of hexadecyltrimethoxysilane were added to 100 mL of deionized water, magnetically stirred for 20 min, ultrasonically treated for 60 min, and then stirred at 60 ° C for 6 h. After the reaction was completed, the reaction product was filtered, washed, and dried to obtain alkylated kaolin;
[0034] (2) Add 1 g of alkylated kaolin and 0.2 g of aminopropyltrimethoxysilane to 100 mL of deionized water, stir magnetically for 30 min, treat ultrasonically for 20 min, and react at 80 °C for 10 h. After the reaction, centrifuge, wash, and dry the reaction product to obtain amino / alkylated kaolin;
[0035] (3) Add 1 g of amino / alkylated kaolin to 50 mL of 1 wt% chelated lithium molybdenum ion solution, stir and react at 90° C. for 10 h. After the reaction is completed, filter, wash and dry the reaction product to obtain a chelated lithium molybdenum ion lubricant additive.
[0036] The prepared additive was added into SF15W-40 lubricating oil at a concentration of 0.13wt%. Example
[0037] A method for preparing a chelated lithium molybdenum ion lubricating oil additive comprises the following steps:
[0038] (1) 1 g of kaolin and 0.05 g of hexadecyltrimethoxysilane were added to 100 mL of deionized water, magnetically stirred for 10 min, ultrasonically treated for 30 min, and then stirred at 40 ° C for 2 h. After the reaction was completed, the reaction product was filtered, washed, and dried to obtain alkylated kaolin;
[0039] (2) Add 1 g of alkylated kaolin and 0.05 g of aminopropyltrimethoxysilane to 100 mL of deionized water, stir magnetically for 15 min, treat ultrasonically for 10 min, and react at 50 °C for 4 h. After the reaction, centrifuge, wash, and dry the reaction product to obtain amino / alkylated kaolin;
[0040] (3) Add 1 g of amino / alkylated kaolin to 30 mL of 0.1 wt% chelated lithium molybdenum ion solution, stir and react at 70 ° C for 6 h. After the reaction is completed, filter, wash and dry the reaction product to obtain a chelated lithium molybdenum ion lubricant additive.
[0041] The prepared additive was added into SF15W-40 lubricating oil at a concentration of 0.01wt%. Example
[0042] A method for preparing a chelated lithium molybdenum ion lubricating oil additive comprises the following steps:
[0043] (1) 1 g of kaolin and 0.2 g of hexadecyltrimethoxysilane were added to 100 mL of deionized water, magnetically stirred for 15 min, ultrasonically treated for 40 min, and then stirred at 50 ° C for 3 h. After the reaction was completed, the reaction product was filtered, washed, and dried to obtain alkylated kaolin;
[0044] (2) adding 1 g of alkylated kaolin and 0.1 g of aminopropyltrimethoxysilane to 100 mL of deionized water, magnetically stirring for 20 min, ultrasonically treating for 15 min, stirring and reacting at 60 ° C for 6 h. After the reaction is completed, the reaction product is centrifuged, washed, and dried to obtain amino / alkylated kaolin;
[0045] (3) Add 1 g of amino / alkylated kaolin to 40 mL of 0.6 wt% chelated lithium molybdenum ion solution, stir and react at 80 ° C for 8 h. After the reaction is completed, filter, wash and dry the reaction product to obtain a chelated lithium molybdenum ion lubricant additive.
[0046] The prepared additive was added into SF15W-40 lubricating oil at a concentration of 0.05wt%. Example
[0047] A method for preparing a chelated lithium molybdenum ion lubricating oil additive comprises the following steps:
[0048] (1) 1 g of kaolin and 0.3 g of hexadecyltrimethoxysilane were added to 100 mL of deionized water, magnetically stirred for 18 min, ultrasonically treated for 50 min, and then stirred at 55 ° C for 5 h. After the reaction was completed, the reaction product was filtered, washed, and dried to obtain alkylated kaolin;
[0049] (2) adding 1 g of alkylated kaolin and 0.15 g of aminopropyltrimethoxysilane to 100 mL of deionized water, magnetically stirring for 25 min, ultrasonically treating for 15 min, stirring and reacting at 70 ° C for 8 h. After the reaction is completed, the reaction product is centrifuged, washed, and dried to obtain amino / alkylated kaolin;
[0050] (3) Add 1 g of amino / alkylated kaolin to 45 mL of 0.8 wt% chelated lithium molybdenum ion solution, stir and react at 80 °C for 9 h. After the reaction is completed, filter, wash and dry the reaction product to obtain a chelated lithium molybdenum ion lubricant additive.
[0051] The prepared additive was added into SF15W-40 lubricating oil at a concentration of 0.1wt%.
[0052] A method for preparing a lubricating oil additive comprises the following steps:
[0053] (1) Add 1 g of kaolin and 0.2 g of aminopropyltrimethoxysilane to 100 mL of deionized water, stir magnetically for 30 min, treat ultrasonically for 20 min, and react at 80 ° C for 10 h. After the reaction, centrifuge, wash, and dry the reaction product to obtain amino kaolin;
[0054] (2) Add 1 g of aminated kaolin to 50 mL of 1 wt% chelated lithium molybdenum ion solution, stir and react at 90° C. for 10 h. After the reaction is completed, filter, wash and dry the reaction product to obtain an additive.
[0055] The prepared additive was added into SF15W-40 lubricating oil at a concentration of 0.13wt%.
[0056] A method for preparing a lubricating oil additive comprises the following steps:
[0057] (1) 1 g of kaolin and 0.5 g of hexadecyltrimethoxysilane were added to 100 mL of deionized water, magnetically stirred for 20 min, ultrasonically treated for 60 min, and then stirred at 60 ° C for 6 h. After the reaction was completed, the reaction product was filtered, washed, and dried to obtain alkylated kaolin;
[0058] (2) Add 1 g of alkylated kaolin to 50 mL of 1 wt% chelated lithium molybdenum ion solution, stir and react at 90° C. for 10 h. After the reaction is completed, filter, wash and dry the reaction product to obtain an additive.
[0059] The prepared additive was added into SF15W-40 lubricating oil at a concentration of 0.13wt%.
[0060] A method for preparing a lubricating oil additive comprises the following steps:
[0061] (1) 1 g of kaolin and 0.5 g of hexadecyltrimethoxysilane were added to 100 mL of deionized water, magnetically stirred for 20 min, ultrasonically treated for 60 min, and then stirred at 60 ° C for 6 h. After the reaction was completed, the reaction product was filtered, washed, and dried to obtain alkylated kaolin;
[0062] (2) Add 1 g of alkylated kaolin and 0.2 g of aminopropyltrimethoxysilane to 100 mL of deionized water, stir magnetically for 30 min, treat ultrasonically for 20 min, and react at 80 °C for 10 h. After the reaction, centrifuge, wash, and dry the reaction product to obtain amino / alkylated kaolin.
[0063] The prepared amino / alkylated kaolin was added into SF15W-40 lubricating oil at a concentration of 0.13 wt%.
[0064] The anti-wear and friction-reducing properties of the lubricating oils prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were investigated using a SGW-10A four-ball friction and wear tester. The experimental steel ball was made of high-quality chromium alloy bearing steel GCr15, with a Rockwell hardness of HRC64 to 66 and a diameter of 12.7 mm. The experimental loading force was 147 N, the speed was 1200 r / min, and the time was 60 min. After the experiment, the steel ball was cleaned and the diameter of the steel ball friction spot after the friction experiment was measured using an optical microscope. The mass loss of the steel ball before and after the experiment was weighed using a one-tenth electronic balance. The test results are shown in Table 1.
[0065] Table 1 Friction coefficient, friction spot diameter and mass loss of different additives in lubricating oil
[0066] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a chelated lithium molybdenum ion lubricating oil additive, characterized in that: The steps include: (1) adding kaolin and hexadecyltrimethoxysilane into deionized water, magnetically stirring, ultrasonically treating, and then stirring to react. After the reaction is completed, filtering, washing, and drying the reaction product to obtain alkylated kaolin; (2) adding alkylated kaolin and aminopropyltrimethoxysilane into deionized water, magnetically stirring, ultrasonically treating, and then stirring to react. After the reaction is completed, centrifuging, washing, and drying the reaction product to obtain amino / alkylated kaolin; (3) adding amino / alkylated kaolin to the chelated lithium molybdenum ion solution, stirring for reaction, and after the reaction is completed, filtering, washing, and drying the reaction product to obtain a chelated lithium molybdenum ion lubricating oil additive; In step (1), the mass volume ratio of kaolin, hexadecyltrimethoxysilane and deionized water is 1 g: 0.05-0.5 g: 100 mL; In step (1), magnetic stirring is performed for 10 to 20 minutes, and ultrasonic treatment is performed for 30 to 60 minutes; the reaction conditions are 40 to 60° C. and 2 to 6 hours; In step (2), the mass volume ratio of alkylated kaolin, aminopropyltrimethoxysilane and deionized water is 1 g: 0.05-0.2 g: 100 mL; In step (2), the magnetic stirring time is 15-30 min, and the ultrasonic treatment time is 10-20 min; the reaction conditions are 50-80° C. and the reaction time is 4-10 h; In step (3), the chemical formula of the chelated lithium molybdenum ion is Li2C 10 H 16 N2O8Mo, the concentration of chelated lithium molybdenum ion solution is 0.1~1wt%; In step (3), the preparation method of the chelated lithium molybdenum ion solution is as follows: weigh EDTA and dissolve it in dilute ammonia water to form an EDTA solution with a concentration of 1 mol / L; weigh lithium acetate and molybdenum nitrate at a molar ratio of EDTA: Li: Mo of 1: 1-2: 0.5-1, add them to the EDTA solution, and stir the reaction at 80° C. for 2 h to obtain a chelated lithium molybdenum ion solution; In step (3), the reaction conditions are stirring the reaction at 70-90° C. for 6-10 hours; the mass volume ratio of amino / alkylated kaolin to chelated lithium molybdenum ion solution is 1 g: 30-50 mL.
2. A lubricating oil additive prepared by the method of claim 1.
3. Use of the additive according to claim 2 in lubricating oil, characterized in that: The concentration of the additive in the lubricating oil is 0.01-0.13 wt %.
4. Use of the additive according to claim 2 in lubricating oil, characterized in that: The lubricating oils include Kunlun Scorpio F5000 lubricating oil, SF15W-40 lubricating oil and Great Wall SJ10W-40 lubricating oil, or mineral base oil and synthetic base oil.