Preparation method and application of ZnCdS / NiO composite photocatalyst
By constructing ZnCdS/NiO composite photocatalyst on the NiO surface, the problem of low carrier separation efficiency of ZnCdS photocatalyst is solved, and high-efficiency photocatalytic hydrogen production is achieved, which reduces preparation cost and energy consumption and improves photocatalytic performance.
Patent Information
- Application Number
- CN202310661785.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-06-06
AI Technical Summary
The existing ZnCdS photocatalysts have problems with low carrier separation efficiency, short life and easy corrosion. The quantum yield of NiO is low, making it difficult to effectively improve the photocatalytic hydrogen production efficiency.
ZnCdS was prepared by hydrothermal method, and it was grown on the NiO surface by solvothermal method to form a heterojunction to form a ZnCdS/NiO composite photocatalyst, and non-precious metal oxide semiconductors were introduced to promote the rapid transfer of photogenerated electrons and provide more active sites point.
The photocatalytic hydrogen production efficiency is significantly improved, the preparation cost of composite catalysts is reduced, the material performance is significantly improved, the energy consumption is low, and the operation is simple. The synthetic composite photocatalytic hydrogen production performance is good.
Smart Images

Figure HDA0004269319340000011 
Figure HDA0004269319340000012 
Figure HDA0004269319340000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and particularly relates to a preparation method of a ZnCdS / NiO composite photocatalyst and application thereof. Background Art
[0002] Population growth and rapid industrialization have led to fossil energy crises and environmental pollution. The development of sustainable energy is playing an increasingly important role. Hydrogen, known as the "future oil", is one of the most promising alternatives as a clean new energy source.
[0003] From the perspective of environment and cost, decomposing water to produce hydrogen through solar energy is a promising way to produce hydrogen. Photocatalytic hydrogen production is an important means of using solar energy to solve energy and environmental problems. The research on photocatalytic hydrogen production technology is at the forefront of high-tech and has received widespread attention in various fields.
[0004] As a ternary sulfide, ZnCdS has a suitable band gap, visible light response, and good photocatalytic activity, and has a good hydrogen production effect. However, since pure ZnCdS has low separation efficiency of photoexcited carriers, short lifetime, and is easily corroded by light, it is particularly important to use ZnCdS to construct heterojunctions. NiO is a stable semiconductor with a large specific surface area, which can provide more active sites and inhibit the aggregation of photogenerated carriers. However, the quantum yield of NiO is low. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention aims to provide a method for preparing a ZnCdS / NiO composite photocatalyst and its application. In the present invention, ZnCdS (ZCS) is first prepared by a hydrothermal method, and then ZCS is grown on the surface of NiO by a solvothermal method to construct a heterojunction and prepare a composite photocatalyst; the ZnCdS / NiO composite photocatalyst can significantly improve the efficiency of photocatalytic hydrogen production.
[0006] The present invention provides a method for preparing a ZnCdS / NiO composite photocatalyst, comprising the following steps:
[0007] S1: dissolving a zinc source, a cadmium source, a sulfur source and sodium hydroxide in deionized water, stirring them fully to react, and washing and drying the reaction product to obtain ZnCdS;
[0008] S2: Mix ZnCdS and deionized water to prepare a ZnCdS suspension, add a nickel source to the ZnCdS suspension, stir until completely dissolved, adjust the pH value of the solution with ammonia water, and then carry out a hydrothermal reaction. After the reaction is completed, cool, centrifuge, wash, and dry to obtain a powder, which is placed in a muffle furnace for calcination. Finally, naturally cool to room temperature, take out and grind thoroughly to obtain a ZnCdS / NiO composite photocatalyst.
[0009] Preferably, the molar ratio of the zinc source, cadmium source and sulfur source in step S1 is 1:(0.5-1):(2-2.5); the zinc source is zinc nitrate hexahydrate, the cadmium source is cadmium acetate dihydrate, and the sulfur source is any one of sodium sulfide or thioacetamide.
[0010] Preferably, the concentration of sodium hydroxide is 2.8-5.5 M, and the alkaline environment provided by sodium hydroxide is conducive to the reaction.
[0011] Preferably, the time for sufficient stirring in step S1 is 0.5-1 h.
[0012] Preferably, the reaction temperature in step S1 is 180-200° C., and the reaction time is 18-24 h.
[0013] Preferably, in step S1, the reactants are centrifuged and washed at a rotation speed of 4000-6000 rpm.
[0014] Preferably, in step S1, the drying temperature is 65° C. and the drying time is 12 h.
[0015] Preferably, in step S2, ZnCdS and deionized water are mixed in a ratio of 1 mg:30 mL to prepare a ZnCdS suspension.
[0016] Preferably, the nickel source in step S2 is NiCl 2 ·2H 2 O, control NiCl 2 ·2H 2 The mass ratio of O to ZnCdS is (3-10):1.
[0017] Preferably, the stirring time in step S2 is 10-30 min.
[0018] Preferably, in step S2, the pH value of the solution is adjusted to 9-11 with aqueous ammonia.
[0019] Preferably, the temperature of the hydrothermal reaction in step S2 is 160° C. and the reaction time is 6 h.
[0020] Preferably, the rotation speed of the centrifugal washing in step S2 is 6000-8000 rpm.
[0021] Preferably, the calcination temperature in step S2 is 250° C., the calcination time is 2 h, and the heating rate is 5° C. / min.
[0022] The preparation method provided by the present invention introduces non-precious metal oxide semiconductors to construct heterojunctions, which can not only promote the rapid transfer of photogenerated electrons, but also provide more active sites; in particular, through photodeposition, ZCS can be more adaptably and evenly deposited on the NiO surface under the induction of photogenerated electrons and holes, thereby significantly improving performance when a small amount of non-precious metal catalysts are introduced. The above-constructed photocatalytic composite catalyst can play a good synergistic role.
[0023] The present invention also provides an application of the ZnCdS / NiO composite photocatalyst prepared by the above method, wherein the ZnCdS / NiO composite photocatalyst is used for photocatalytic hydrogen production, comprising: performing the process in a closed vacuum apparatus (CEL-PAEM-D8), controlling the temperature of the reactor at 7-8°C by a water cooling system. Add 20 mg of the prepared ZnCdS / NiO composite photocatalyst to 100 mL of a solution (0.35 mol / L sodium sulfide solution and 0.25 mol / L sodium sulfite solution), obtain a uniform suspension by ultrasonic crushing, place the above solution in a 200 ml quartz reactor, fix the reactor containing the solution on the reactor, and fill the sealed reactor with nitrogen. Under the irradiation of a xenon lamp, use a gas chromatograph (Agilent GC7820A) to detect H in the gas phase every 30 minutes. 2 Finally, real-time data was obtained through professional software (IBrainChrom).
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] 1. The preparation method provided by the present invention constructs a ZnCdS / NiO heterojunction, which allows rapid transfer of electrons generated by light excitation, can reduce a portion of the recombination of photogenerated carriers, and significantly improves the photocatalytic performance of the material.
[0026] 2. The present invention only needs to load a small amount of non-precious metal oxide semiconductor to achieve significant performance improvement, greatly reducing the preparation cost of the composite catalyst.
[0027] 3. The present invention uses a calcination-hydrothermal method to allow ZnCdS nanoparticles to be more adaptably and uniformly deposited or grown on the surface of NiO nanosheets under the induction of photogenerated electrons and holes.
[0028] 4. The preparation method provided by the present invention requires a relatively low reaction temperature, which reduces energy consumption and makes the experimental process safer. The reaction raw materials are simple and easy to obtain, the required energy consumption is small, and the operation is simple. The synthesized composite photocatalyst has good photocatalytic hydrogen production performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 XRD spectra of ZnCdS, NiO and ZCS / NiO composite photocatalysts.
[0030] Figure 2 This is the SEM image of ZCS / NiO composite photocatalyst.
[0031] Figure 3 The hydrogen production rate diagram of the ZCS / NiO composite photocatalyst prepared in Example 1-4 and ZCS and NiO;
[0032] Figure 4 This is a graph of the hydrogen production rate of the ZCS / NiO composite photocatalyst prepared in Example 3, Example 5 and Example 6. DETAILED DESCRIPTION
[0033] The present invention is not limited to the following specific embodiments, and the following detailed descriptions are all illustrative and are intended to provide further explanation of the present application. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by ordinary technicians in the technical field to which the present application belongs.
[0034] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.
[0035] Example 1
[0036] A method for preparing a ZnCdS / NiO composite photocatalyst, comprising the following steps:
[0037] S1: Dissolve zinc nitrate hexahydrate, cadmium acetate dihydrate and thioacetamide in a molar ratio of 2:2:5 in deionized water respectively, add deionized water and stir for 10 minutes after mixing; dissolve 0.4mmol of NaOH solid in 10mL of deionized water, add to the above mixed solution, mix evenly, and stir for 30 minutes; then transfer the mixture to a polytetrafluoroethylene reactor and react at 180℃ for 20h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for multiple times, and dry at 65℃ to obtain ZnCdS.
[0038] S2: Dissolve 0.476g of the prepared ZnCdS in deionized water to obtain a suspension; dissolve 1.43g of nickel chloride dihydrate in the above suspension to form a light green solution; then add ammonia water to adjust the pH value of the solution to 11; then transfer the mixed solution to a polytetrafluoroethylene reactor and react at 160°C for 6h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for multiple times; dry at 60°C and grind; then transfer the ground solid black powder to a crucible and react at 250°C for 2h with a heating rate of 5°C / min; grind after the reaction to obtain a ZnCdS / NiO composite photocatalyst (labeled as ZCS / NiO-1).
[0039] Example 2
[0040] A method for preparing a ZnCdS / NiO composite photocatalyst, comprising the following steps:
[0041] S1: Dissolve zinc nitrate hexahydrate, cadmium acetate dihydrate and thioacetamide in a molar ratio of 2:2:5 in deionized water, add deionized water and stir for 10 minutes after mixing; dissolve 0.4mmol of NaOH solid in 10mL of deionized water, add it to the above mixed solution and mix evenly, stir for 30 minutes; then transfer the mixture to a polytetrafluoroethylene reactor and react at 180℃ for 20h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for many times, and dry at 65℃ to obtain ZnCdS. X-ray diffraction test results are shown in Figure 1 .
[0042] S2: Dissolve 0.286g of the prepared ZnCdS in deionized water to obtain a suspension; dissolve 1.43g of nickel chloride dihydrate in the above suspension to form a light green solution; then add ammonia water to adjust the pH value of the solution to 11; then transfer the mixed solution to a polytetrafluoroethylene reactor and react at 160°C for 6h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for multiple times; dry at 60°C and grind; then transfer the ground solid black powder to a crucible and react at 250°C for 2h with a heating rate of 5°C / min; after the reaction, grind to obtain a ZnCdS / NiO composite photocatalyst (labeled as ZCS / NiO-2).
[0043] Example 3
[0044] A method for preparing a ZnCdS / NiO composite photocatalyst, comprising the following steps:
[0045] S1: Dissolve zinc nitrate hexahydrate, cadmium acetate dihydrate and thioacetamide in a molar ratio of 2:2:5 in deionized water respectively, add deionized water and stir for 10 minutes after mixing; dissolve 0.4mmol of NaOH solid in 10mL of deionized water, add to the above mixed solution, mix evenly, and stir for 30 minutes; then transfer the mixture to a polytetrafluoroethylene reactor and react at 180℃ for 20h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for multiple times, and dry at 65℃ to obtain ZnCdS.
[0046] S2: Dissolve 0.17875g of the prepared ZnCdS in deionized water to obtain a suspension; dissolve 1.43g of nickel chloride dihydrate in the above suspension to form a light green solution; then add ammonia water to adjust the pH value of the solution to 11; then transfer the mixed solution to a polytetrafluoroethylene reactor and react at 160°C for 6h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for multiple times; dry at 65°C and grind; then transfer the ground solid black powder to a crucible and react at 250°C for 2h with a heating rate of 5°C / min; grind after the reaction to obtain a ZnCdS / NiO composite photocatalyst (labeled as ZCS / NiO-3).
[0047] Example 4
[0048] A method for preparing a ZnCdS / NiO composite photocatalyst, comprising the following steps:
[0049] S1: Dissolve zinc nitrate hexahydrate, cadmium acetate dihydrate and thioacetamide in a molar ratio of 2:2:5 in deionized water respectively, add deionized water and stir for 10 minutes after mixing; dissolve 0.4mmol of NaOH solid in 10mL of deionized water, add to the above mixed solution, mix evenly, and stir for 30 minutes; then transfer the mixture to a polytetrafluoroethylene reactor and react at 180℃ for 20h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for multiple times, and dry at 65℃ to obtain ZnCdS.
[0050] S2: Dissolve 0.143g of the prepared ZnCdS in deionized water to obtain a suspension; dissolve 1.43g of nickel chloride dihydrate in the above suspension to form a light green solution; then add ammonia water to adjust the pH value of the solution to 11; then transfer the mixed solution to a polytetrafluoroethylene reactor and react at 160°C for 6h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for multiple times; dry at 65°C and grind; then transfer the ground solid black powder to a crucible and react at 250°C for 2h with a heating rate of 5°C / min; grind after the reaction to obtain a ZnCdS / NiO composite photocatalyst (labeled as ZCS / NiO-4).
[0051] Example 5
[0052] A method for preparing a ZnCdS / NiO composite photocatalyst, comprising the following steps:
[0053] S1: Dissolve zinc nitrate hexahydrate, cadmium acetate dihydrate and thioacetamide in a molar ratio of 2:2:5 in deionized water respectively, add deionized water and stir for 10 minutes after mixing; dissolve 0.3mmol of NaOH solid in 10mL of deionized water, add it to the above mixed solution, mix evenly, and stir for 30 minutes; then transfer the mixture to a polytetrafluoroethylene reactor and react at 180℃ for 20h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for multiple times, and dry at 65℃ to obtain ZnCdS.
[0054] S2: Dissolve 0.17875g of the prepared ZnCdS in deionized water to obtain a suspension; dissolve 1.43g of nickel chloride dihydrate in the above suspension to form a light green solution; add ammonia water to adjust the pH value of the solution to 11; then transfer the mixed solution to a polytetrafluoroethylene reactor and react at 160°C for 6h; after the reaction, cool to room temperature and wash with pure water and ethanol by centrifugation for multiple times; dry at 60°C and grind; then transfer the ground solid black powder to a crucible and react at 250°C for 2h with a heating rate of 5°C / min; grind after the reaction to obtain a ZnCdS / NiO composite photocatalyst (labeled as ZCS / NiO-5).
[0055] Example 6
[0056] A method for preparing a ZnCdS / NiO composite photocatalyst, comprising the following steps:
[0057] S1: Dissolve zinc nitrate hexahydrate, cadmium acetate dihydrate and thioacetamide in a molar ratio of 2:2:5 in deionized water respectively, add deionized water and stir for 10 minutes after mixing; dissolve 0.5mmol of NaOH solid in 10mL of deionized water, add it to the above mixed solution, mix evenly, and stir for 30 minutes; then transfer the mixture to a polytetrafluoroethylene reactor and react at 180℃ for 20h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for multiple times, and dry at 65℃ to obtain ZnCdS.
[0058] S2: Dissolve 0.17875g of the prepared ZnCdS in deionized water to obtain a suspension; dissolve 1.43g of nickel chloride dihydrate in the above suspension to form a light green solution; then add ammonia water to adjust the pH value of the solution to 11; then transfer the mixed solution to a polytetrafluoroethylene reactor and react at 160°C for 6h; after the reaction, cool to room temperature, wash with pure water and ethanol by centrifugation for multiple times; dry at 65°C and grind; then transfer the ground solid black powder to a crucible and react at 250°C for 2h with a heating rate of 5°C / min; grind after the reaction to obtain a ZnCdS / NiO composite photocatalyst (labeled as ZCS / NiO-6).
[0059] Comparative Example 1
[0060] A method for preparing a NiO photocatalyst, comprising the following steps:
[0061] 1.43g nickel chloride dihydrate was dissolved in 30mL deionized water to obtain a light green solution, and then ammonia water was added to adjust the solution pH to 11, and ultrasonic and fully stirred. The mixed solution was then transferred to a polytetrafluoroethylene reactor and reacted at 160°C for 6h; after the reaction, it was cooled to room temperature and washed several times by centrifugation with pure water and ethanol; dried at 65°C and ground; then the ground solid black powder was transferred to a crucible and reacted at 250°C for 2h with a heating rate of 5°C / min to obtain NiO.
[0062] Figure 1 Figure 2 is the XRD spectra of ZCS, NiO and ZCS / NiO composite photocatalyst. It can be seen that the X-ray diffraction peak of ZCS / NiO contains the characteristic peaks of ZCS and NiO, which indicates the successful preparation of ZCS / NiO composite photocatalyst.
[0063] Figure 2 This is the SEM image of the ZCS / NiO composite photocatalyst. It can be seen that the ZCS nanoparticles are attached to the surface of the NiO nanosheets.
[0064] Figure 3 The hydrogen production rate diagram of the ZCS / NiO composite photocatalyst prepared in Examples 1-4 and ZCS and NiO shows that the hydrogen production rate of the ZCS / NiO composite photocatalyst is much higher than that of ZCS and NiO, among which the ZCS / NiO-3 prepared in Example 3 has the best hydrogen production effect.
[0065] Figure 4 This is a graph of the hydrogen production rate of the ZCS / NiO composite photocatalyst prepared in Example 3, Example 5 and Example 6. It can be seen from the graph that when the concentration of the NaOH solution is 0.4 mol / L, the hydrogen production effect of the prepared ZCS / NiO composite photocatalyst is the best.
Claims
1. A method for preparing a ZnCdS / NiO composite photocatalyst, characterized in that: The following steps are involved: S1: dissolving a zinc source, a cadmium source, a sulfur source and sodium hydroxide in deionized water, stirring them fully and reacting them, washing and drying the reaction product to obtain ZnCdS; the molar ratio of the zinc source, the cadmium source and the sulfur source is 1:1:2.5; the amount of the sodium hydroxide is 0.4 mmol; the reaction temperature is 180°C, and the reaction time is 20 h; S2: ZnCdS is mixed with deionized water to prepare a ZnCdS suspension, a nickel source is added to the ZnCdS suspension, and the mixture is stirred until completely dissolved. The pH value of the solution is adjusted to 11 with aqueous ammonia, and then a hydrothermal reaction is carried out. After the reaction is completed, the mixture is cooled, centrifuged, washed, and dried to obtain a powder, which is placed in a muffle furnace for calcination. Finally, the mixture is naturally cooled to room temperature, taken out and fully ground to obtain a ZnCdS / NiO composite photocatalyst; the nickel source is NiCl2▪2H2O, and the mass ratio of NiCl2▪2H2O to ZnCdS is controlled to be 5:1; the calcination temperature is 250°C, the calcination time is 2h, and the heating rate is 5°C / min.
2. The method for preparing the ZnCdS / NiO composite photocatalyst according to claim 1, characterized in that: In step S1, the zinc source is zinc nitrate hexahydrate, the cadmium source is cadmium acetate dihydrate, and the sulfur source is sodium sulfide or thioacetamide.
3. The method for preparing the ZnCdS / NiO composite photocatalyst according to claim 1, characterized in that: The time for sufficient stirring in step S1 is 0.5-1h; And / or, the washing in step S1: washing the reactants by centrifugation at a speed of 4000-6000 rpm; And / or, the drying in step S1: the drying temperature is 65° C. and the drying time is 12 h.
4. The method for preparing the ZnCdS / NiO composite photocatalyst according to claim 1, characterized in that: In step S2, ZnCdS and deionized water are mixed in a ratio of 1 mg:30 mL to prepare a ZnCdS suspension.
5. The method for preparing the ZnCdS / NiO composite photocatalyst according to claim 1, characterized in that: The stirring time in step S2 is 10-30 min; And / or, the temperature of the hydrothermal reaction in step S2 is 160° C. and the reaction time is 6 h; And / or, the rotation speed of the centrifugal washing in step S2 is 6000-8000 rpm.