A Mn-doped PIN-PSN-PT hard piezoelectric ceramic and its preparation method

By using the B-site cationic precursor method and high-temperature solid-state reaction synthesis method of Mn-doped PIN-PSN-PT ceramics in hard piezoelectric ceramics, the material system and phase structure are optimized, and the high-power problems of existing hard piezoelectric ceramics are solved. The problem of insufficient heat generation and temperature stability in the device has been achieved, and the improvement of high mechanical quality factor, piezoelectric coefficient and Curie temperature has been achieved.

CN116715523BActive Publication Date: 2024-10-29XI AN JIAOTONG UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310711939.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-15
Publication Date
2024-10-29
Estimated Expiration
2043-06-15

AI Technical Summary

Technical Problem

Existing hard piezoelectric ceramics have problems such as severe heating, low output and small operating temperature range in high-power piezoelectric devices. Moreover, the performance parameters restrict each other, making it difficult to simultaneously meet the high mechanical quality factor, high voltage electrical coefficient and high Curie temperature. requirements.

Method used

Mn-doped PIN-PSN-PT hard piezoelectric ceramics and its preparation method are used, and the material system is optimized through the B-site cation precursor method combined with the high-temperature solid-state reaction synthesis method, and In and Sc elements are selected to replace the Zr element in the traditional PZT system. , and carry out Mn element doping to adjust the phase structure to form a pure ABO3 type perovskite structure without pyrochlore phase.

Benefits of technology

Ceramics that achieve high mechanical quality factor, high piezoelectric coefficient and high Curie temperature improve temperature stability and output performance and are suitable for high-power piezoelectric devices. The piezoelectric coefficient can reach up to 381pC/N, and the mechanical quality factor can reach up to 381pC/N. reaches 2828, and the Curie temperature can reach up to 300°C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116715523B_ABST
    Figure CN116715523B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of piezoelectric ceramic materials, and specifically relates to a Mn-doped PIN-PSN-PT hard piezoelectric ceramic and a preparation method thereof. The composition formula of the hard piezoelectric ceramic is (1-x-y)Pb(In 1 / 2 Nb 1 / 2 )O3‑xPb(Sc 1 / 2 Nb 1 / 2 )O3‑yPbTiO3‑zMn, wherein 0.385≤x≤0.405, 0.405≤y≤0.425, 0.015≤z≤0.025. Firstly, ScNbO4 and InNbO4 precursor powders are synthesized by the B-site cation precursor method, and then ScNbO4, InNbO4, TiO2, manganese source and lead source are used as raw materials, and PIN‑PSN‑PT‑Mn powders are obtained by calcination. Finally, the hard piezoelectric ceramics are obtained through grinding and granulation, dry pressing, debinding sintering, silver polarization and other processes. Through material system optimization and phase structure regulation, the mutual constraints between the performance parameters of piezoelectric materials are effectively weakened, and the trigonal‑tetragonal ferroelectric phase transition temperature is controlled below room temperature. m and high d 33 At the same time, it can maintain good temperature stability and is expected to be widely used in high-power piezoelectric devices such as resonant piezoelectric motors, piezoelectric transformers, and ultrasonic transducers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of piezoelectric ceramic materials, and in particular relates to a Mn-doped PIN-PSN-PT hard piezoelectric ceramic and a preparation method thereof. Background Art

[0002] Piezoelectric material is an electronic functional material that can realize the mutual conversion between mechanical energy and electrical energy. It has a crystal structure in which the positive and negative charge centers do not overlap, and can generate a potential difference under the action of external stress, or generate strain under the action of an external voltage. Piezoelectric ceramics are currently the most widely used piezoelectric material due to their advantages such as low cost, easy preparation, and convenient performance regulation. By doping with low-cost acceptor elements, under the pinning effect of oxygen vacancies and defect dipoles on domain wall motion, hard piezoelectric ceramics with high mechanical quality factor and low dielectric loss can be obtained, which are suitable for use in high-power energy conversion fields, such as drivers, transformers, ultrasonic transducers, etc.

[0003] Piezoelectric materials commonly used in high-power piezoelectric devices need to have both high Q m , high d 33 and high T c The characteristics of the PZT system in commercial use are difficult to obtain in the case of high Q m While still maintaining high d 33 (PZT-8 Ceramic Q m ≈1200,d 33 ≈240pC / N). In recent years, researchers have proposed a variety of new hard piezoelectric ceramics, but the inherent mutual constraints of piezoelectric materials limit the application of these products in high-power devices. For example, a Sr, Ce, Cu, Nb doped PMN-PZT system hard piezoelectric ceramic has a mechanical quality factor of less than 1300 (patent number ZL202210933958.0); a Bi, Sb and rare earth element doped PZT system hard piezoelectric ceramic has a mechanical quality factor of less than 1800, and when Q m At maximum, d 33 Less than 320pC / N (patent number ZL202111599985.0); A PMN-PT system hard piezoelectric ceramic for power transducers 33 Higher, but Q mLess than 1000, and the Curie temperature of this ceramic is relatively low, only 130°C (patent number ZL202110615534.5). Generally, the operating temperature of piezoelectric ceramics should not exceed 1 / 2 of the Curie temperature. Therefore, when the temperature exceeds 65°C, the performance of this ceramic will deteriorate. In 2019, researchers proposed an undoped PIN-PSN-PT textured ceramic (Chinese patent application number 201910930606.8), whose Curie temperature is 262°C, which is a high T c The preparation of piezoelectric ceramics provides a way of thinking, but this undoped textured ceramic is a soft ceramic with a low Q m , high dielectric loss and strain hysteresis as well as complex texturing process limit its application areas and production efficiency. In addition, this kind of ceramic has a rhombohedral-tetragonal ferroelectric phase transition in the range of room temperature to Curie temperature. The performance of the ceramic will fluctuate greatly near the phase transition point, which will greatly reduce the temperature stability.

[0004] Studies have shown that due to the influence of factors such as material density, grain size, domain structure, and intrinsic lattice strain, the mutual constraints between the various performance parameters of piezoelectric materials are different in different components or systems. Only by systematically optimizing the material system can its comprehensive performance be effectively improved. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a Mn-doped PIN-PSN-PT hard piezoelectric ceramic and a preparation method thereof. The prepared hard piezoelectric ceramic has both high mechanical quality factor and high piezoelectric coefficient, and can maintain good temperature stability, thereby solving the problems of severe heat generation, low output, and small operating temperature range that exist in existing hard piezoelectric ceramics when applied to high-power piezoelectric devices.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is: a Mn-doped PIN-PSN-PT hard piezoelectric ceramic, wherein the Mn-doped hard piezoelectric ceramic has the following general composition formula: (1-xy)Pb(In 1 / 2 Nb 1 / 2 )O3-xPb(Sc 1 / 2Nb 1 / 2 )O3-yPbTiO3-zMn, among which, 0.385≤x≤0.405, 0.405≤y≤0.425, 0.015≤z≤0.025.

[0007] It is a pure ABO3 perovskite structure without pyrochlore phase.

[0008] At the same time, a preparation method of the Mn-doped PIN-PSN-PT hard piezoelectric ceramic of the invention is provided, which is prepared by a B-site cation precursor method combined with a high-temperature solid-phase reaction synthesis method, and specifically comprises the following steps:

[0009] Step 1, according to the chemical formula (1-xy)Pb(In 1 / 2 Nb 1 / 2 )O3-xPb(Sc 1 / 2 Nb 1 / 2 )O3-yPbTiO3-zMn stoichiometric ratio ScNbO4 precursor powder, InNbO4 precursor powder, TiO2, manganese source and lead source were weighed, ball milled and mixed evenly and dried, and then calcined at 800-900℃ for 1-8h to obtain Pb(In 1 / 2 Nb 1 / 2 )O3-Pb(Sc 1 / 2 Nb 1 / 2 )O3-PbTiO3-Mn powder;

[0010] Step 2: Pb(In 1 / 2 Nb 1 / 2 )O3-Pb(Sc 1 / 2 Nb 1 / 2 ) O3-PbTiO3-Mn powder is put into a ball mill, and after being evenly mixed and dried, 1wt%-2wt% of polyvinyl alcohol is added as a binder, granulated and sieved, and dry-pressed at a pressure of 2-10MPa to obtain a ceramic green body;

[0011] Step 3, placing the ceramic green body in PIN-PSN-PT powder, placing a lead compensation sheet 1-3 cm away from the green body, and covering the crucible to provide a lead-rich atmosphere; after heating, debinding and sintering, the Mn-doped PIN-PSN-PT hard piezoelectric ceramic is obtained.

[0012] The preparation of ScNbO4 and InNbO4 precursor powders includes the following steps: weighing a scandium source, an indium source and a niobium source according to the stoichiometric ratio of the chemical formula ScNbO4 and InNbO4, respectively, mixing them evenly by ball milling, drying the evenly mixed raw materials, and calcining them at 1150-1250°C and 1050-1150°C for 1-8h, respectively, to obtain ScNbO4 precursor powder and InNbO4 precursor powder.

[0013] The scandium source, indium source, niobium source and lead source are Sc 3+ 、In 3+ , Nb 5+ , Pb 2+ The corresponding carbonate, acetate, hydroxide, nitrate, oxalate or oxide, the manganese source can be Mn 2+ , Mn 3+ or Mn 4+ The corresponding carbonates, acetates, hydroxides, nitrates, oxalates or oxides.

[0014] The preparation method of the lead compensation sheet in step 3 is: first weigh PbO and ZrO2 according to a stoichiometric ratio of 1:1, mix them by ball milling, dry the discharged materials and directly dry-press them under a pressure of 2-10MPa to obtain the lead compensation sheet.

[0015] In step 3, the ceramic green body is placed in PIN-PSN-PT powder of the same mass and composition as the green body, and the mass of the lead compensation sheet is 1 / 4-1 / 2 of the mass of the green body.

[0016] In step 3, the temperature is first kept at 550°C-650°C for 1-8 hours for debinding, and then the temperature is increased to 1200-1300°C at a heating rate of 3-5°C / min and kept for 2-4 hours for sintering.

[0017] Compared with the prior art, the present invention has at least the following beneficial effects:

[0018] Based on the optimization of material system, doping modification and phase structure regulation, the present invention adopts the B-site cation precursor method combined with the high-temperature solid phase reaction synthesis method to prepare the Mn-doped PIN-PSN-PT hard piezoelectric ceramic, which is a pure ABO3 perovskite structure without pyrochlore phase and has high Q m , high T c , high d 33 First, through the optimization of the material system, In and Sc were selected to replace the Zr element in the traditional PZT system, and Mn was doped, which effectively weakened the Q of the traditional PZT system hard piezoelectric ceramics. m , T c ,d 33 The mutual restraint relationship between the performance parameters can increase the output and improve the operating temperature range while solving the serious heating problem of high-power piezoelectric devices; secondly, by changing the PT component content to regulate the phase structure, a ceramic at the phase boundary or tetragonal phase at room temperature can be obtained, and the rhombic-tetragonal ferroelectric phase transition temperature can be reduced to below room temperature, thereby greatly improving the temperature stability of hard piezoelectric ceramics near room temperature. The performance test results show that the piezoelectric coefficient of the ceramic of the present invention can reach up to 381pC / N, and the mechanical quality factor can reach up to 2828, which are 65% and 135% higher than commercial PZT-8 hard piezoelectric ceramics, respectively. At the same time, its Curie temperature can reach up to 300℃, and the dielectric loss is as low as 2.4‰, indicating that this is a hard piezoelectric ceramic with excellent performance, which is expected to be widely used in high-power piezoelectric devices such as resonant piezoelectric motors, piezoelectric transformers, and ultrasonic transducers. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The XRD diffraction patterns of the ceramic materials prepared in Examples 1, 2 and 3 of the present invention.

[0020] Figure 2 This is a scanning electron microscope image of the ceramic material prepared in Example 1 of the present invention.

[0021] Figure 3 This is a graph showing how the dielectric constant and dielectric loss of the ceramic material prepared in Example 2 of the present invention vary with temperature.

[0022] Figure 4 These are the electrostrain curves of the ceramic materials prepared in Examples 1, 2, and 3 of the present invention. DETAILED DESCRIPTION

[0023] The present invention considers that when optimizing the material system: selecting a PT-based relaxor ferroelectric system with a B-site composite cation structure, increasing the number of solid solution components and performing Mn element doping modification can weaken Q m ,d 33 and T c The mutual restraint relationship between them is to obtain high Q m , high d 33 and high T c hard piezoelectric ceramics; on this basis, combined with component fine-tuning and changing the phase structure of the ceramics, ceramics at the phase boundary or tetragonal phase at room temperature can be obtained, and the rhombohedral-tetragonal ferroelectric phase transition temperature can be lowered to below room temperature, thereby improving the temperature stability of the ceramics, which is beneficial to its application in high-power piezoelectric devices.

[0024] The present invention is further described in detail below in conjunction with specific embodiments.

[0025] Example 1

[0026] A high Q m , high T c , high d 33 The hard piezoelectric ceramic and the preparation method thereof, the specific steps are:

[0027] (1) Sc2O3, In2(CO3)3, and Nb2O5 are used as raw materials, weighed according to the stoichiometric ratio of ScNbO4 and InNbO4, and placed in a polytetrafluoroethylene ball mill. Anhydrous ethanol is used as the grinding medium and ZrO2 is used as the grinding ball. The ball mill is milled at a speed of 400 r / min for 12 h. The resulting slurry is then placed in an oven and dried at 100°C for 5 h. After drying, the slurry is sieved through a 40-mesh sieve. The sieved powder is placed in an alumina crucible and calcined. ScNbO4 is calcined at 1150°C for 1 h and InNbO4 is calcined at 1050°C for 1 h to obtain ScNbO4 and InNbO4 precursor powders.

[0028] (2) Taking x = 0.405, y = 0.405, z = 0.015, ScNbO4, InNbO4, TiO2, MnCO3, PbO as raw materials, according to 0.19Pb(In 1 / 2Nb 1 / 2 )O3-0.405Pb(Sc 1 / 2 Nb 1 / 2 )O3-0.405PbTiO3-0.015Mn with a stoichiometric ratio, put into a polytetrafluoroethylene ball mill, use anhydrous ethanol as the grinding medium and ZrO2 as the grinding balls, and ball mill for 12 hours at a speed of 400r / min. Then, the obtained slurry is placed in an oven and baked at 100°C for 5 hours. After drying, it is sieved through a 40-mesh sieve, and the sieved powder is placed in an alumina crucible and calcined at 800°C for 1 hour to obtain PIN-PSN-PT-Mn powder.

[0029] (3) The obtained PIN-PSN-PT-Mn powder is placed in a ball mill and ball milled again under the same ball milling conditions as in (1) and (2). The obtained slurry is then placed in an oven and baked at 100°C for 5 h. After drying, 1 wt% of polyvinyl alcohol (PVA) is added to the powder as a binder and granulated manually, passed through an 80-mesh sieve, and then 0.8 g of the sieved powder is weighed and dry-pressed at 2 MPa to obtain a ceramic green body. The ceramic green body is in the form of a disc with a diameter of 10 mm and a thickness of 1.8 mm.

[0030] (4) The ceramic green body is placed on an alumina ceramic plate covered with a sealed crucible, and the bottom, sides and top of the green body are filled with PIN-PSN-PT powder of the same mass and composition as the green body. A lead compensation sheet with a mass of 1 / 4 of the green body mass is placed 1 cm away from the green body to provide a lead-rich atmosphere. First, the binder is removed at 550°C for 1h, and then the temperature is increased to 1300°C at a heating rate of 3°C / min and sintered for 2h to obtain Mn-doped PIN-PSN-PT ceramics.

[0031] (5) The obtained Mn-doped PIN-PSN-PT ceramic was polished into a disc with a thickness of 0.8 mm, a conductive silver paste was brushed on the surface, and then it was placed on an alumina ceramic plate and silver was sintered at 500°C for 20 min. Thereafter, a high-temperature polarization treatment was performed under a DC electric field of 20 kV / cm for 20 min at a polarization temperature of 100°C. After standing for one week for aging, a Mn-doped PIN-PSN-PT hard piezoelectric ceramic material was obtained.

[0032] The preparation method of the lead compensation sheet in step (4) is as follows: first weigh PbO and ZrO2 according to a stoichiometric ratio of 1:1, mix them by ball milling, dry the discharged materials, and then directly dry press them under a uniaxial pressure of 2 MPa.

[0033] The performance test results show that the hard piezoelectric ceramic material prepared in this embodiment is a pure ABO3 perovskite phase without pyrochlore phase, and its piezoelectric coefficient is 368pC / N, the mechanical quality factor is 2632, the Curie temperature is 285°C, and the dielectric loss is 3.6‰.

[0034] Example 2

[0035] A high Q m , high T c , high d 33 The hard piezoelectric ceramic and the preparation method thereof, the specific steps are:

[0036] (1) Sc(CH3COO)3, In2O3, and Nb2(CO3)5 are used as raw materials, weighed according to the stoichiometric ratio of ScNbO4 and InNbO4, and placed in a polytetrafluoroethylene ball mill. Anhydrous ethanol is used as the grinding medium and ZrO2 is used as the grinding ball. The ball mill is milled at a speed of 400 r / min for 12 h. The resulting slurry is then placed in an oven and dried at 100°C for 5 h. After drying, it is sieved through a 40-mesh sieve and the sieved powder is placed in an alumina crucible for calcination. ScNbO4 is calcined at 1200°C for 5 h and InNbO4 is calcined at 1100°C for 5 h to obtain ScNbO4 and InNbO4 precursor powders.

[0037] (2) Taking x = 0.405, y = 0.405, z = 0.02, ScNbO4, InNbO4, TiO2, MnO2, Pb(CH3COO)2 as raw materials, 0.19Pb(In 1 / 2 Nb 1 / 2 )O3-0.405Pb(Sc 1 / 2 Nb 1 / 2 )O3-0.405PbTiO3-0.02Mn were weighed in a stoichiometric ratio and put into a polytetrafluoroethylene ball mill. Anhydrous ethanol was used as the grinding medium and ZrO2 was used as the grinding balls. The milling was carried out at a speed of 400r / min for 12h. The resulting slurry was then placed in an oven and dried at 100°C for 5h. After drying, the slurry was sieved through a 40-mesh sieve. The sieved powder was placed in an alumina crucible and calcined at 850°C for 5h to obtain PIN-PSN-PT-Mn powder.

[0038] (3) The obtained PIN-PSN-PT-Mn powder is placed in a ball mill and ball milled again under the same ball milling conditions as in (1) and (2). The obtained slurry is then placed in an oven and baked at 100°C for 5 h. After drying, 2 wt% of polyvinyl alcohol (PVA) is added to the powder as a binder and granulated manually, passed through an 80-mesh sieve, and then 0.8 g of the sieved powder is weighed and dry-pressed at 5 MPa to obtain a ceramic green body. The ceramic green body is in the form of a disc with a diameter of 10 mm and a thickness of 1.8 mm.

[0039] (4) The ceramic green body is placed on an alumina ceramic plate covered with a sealed crucible, and the bottom, sides and top of the green body are filled with PIN-PSN-PT powder of the same mass and composition as the green body. A lead compensation sheet with a mass of 1 / 2 of the green body mass is placed 2 cm away from the green body to provide a lead-rich atmosphere. First, the binder is removed at 600°C for 5h, and then the temperature is increased to 1300°C at a heating rate of 4°C / min and sintered for 4h to obtain Mn-doped PIN-PSN-PT ceramics.

[0040] (5) The obtained Mn-doped PIN-PSN-PT ceramic was polished into a disc with a thickness of 0.8 mm, and a conductive silver paste was brushed on the surface. Then, the disc was placed on an alumina ceramic plate and silver was sintered at 550°C for 30 min. After that, a high-temperature polarization treatment was performed under a DC electric field of 30 kV / cm for 30 min at a polarization temperature of 110°C. After standing for one week for aging, a Mn-doped PIN-PSN-PT hard piezoelectric ceramic material was obtained.

[0041] The preparation method of the lead compensation sheet in step (4) is as follows: first weigh PbO and ZrO2 according to a stoichiometric ratio of 1:1, mix them by ball milling, dry the discharged materials, and then directly dry press them under a uniaxial pressure of 5 MPa.

[0042] The performance test results show that the hard piezoelectric ceramic material prepared in this embodiment is a pure ABO3 perovskite phase without pyrochlore phase, and its piezoelectric coefficient is 326pC / N, the mechanical quality factor is 2828, the Curie temperature is 293°C, and the dielectric loss is 2.4‰.

[0043] Example 3

[0044] A high Q m , high T c , high d 33 The hard piezoelectric ceramic and the preparation method thereof, the specific steps are:

[0045] (1) Sc2(CO3)3, In(CH3COO)3, and NbO(NO3)3 are used as raw materials, weighed according to the stoichiometric ratio of ScNbO4 and InNbO4, and placed in a polytetrafluoroethylene ball mill. Anhydrous ethanol is used as the grinding medium and ZrO2 is used as the grinding ball. The ball mill is milled at a speed of 400 r / min for 12 h. The resulting slurry is then placed in an oven and dried at 100°C for 5 h. After drying, the slurry is sieved through a 40-mesh sieve and the sieved powder is placed in an alumina crucible for calcination. ScNbO4 is calcined at 1250°C for 8 h and InNbO4 is calcined at 1150°C for 8 h to obtain ScNbO4 and InNbO4 precursor powders.

[0046] (2) Taking x = 0.395, y = 0.415, z = 0.025, ScNbO4, InNbO4, TiO2, Mn(NO3)2, PbCO3 as raw materials, 0.19Pb(In 1 / 2 Nb 1 / 2 )O3-0.395Pb(Sc 1 / 2 Nb 1 / 2 )O3-0.415PbTiO3-0.025Mn with a stoichiometric ratio, put into a polytetrafluoroethylene ball mill, use anhydrous ethanol as the grinding medium and ZrO2 as the grinding balls, and ball mill for 12 hours at a speed of 400r / min. Then, the obtained slurry is placed in an oven and dried at 100°C for 5 hours. After drying, it is sieved through a 40-mesh sieve, and the sieved powder is placed in an alumina crucible and calcined at 900°C for 8 hours to obtain PIN-PSN-PT-Mn powder.

[0047] (3) The obtained PIN-PSN-PT-Mn powder is placed in a ball mill and ball milled again under the same ball milling conditions as in (1) and (2). The obtained slurry is then placed in an oven and baked at 100°C for 5 h. After drying, 1 wt% of polyvinyl alcohol (PVA) is added to the powder as a binder and granulated manually, passed through an 80-mesh sieve, and then 0.8 g of the sieved powder is weighed and dry-pressed at 10 MPa to obtain a ceramic green body. The ceramic green body is in the form of a disc with a diameter of 10 mm and a thickness of 1.8 mm.

[0048] (4) The ceramic green body is placed on an alumina ceramic plate covered with a sealed crucible, and the bottom, sides and top of the green body are filled with PIN-PSN-PT powder of the same mass and composition as the green body. A lead compensation sheet with a mass of 1 / 4 of the green body mass is placed 3 cm away from the green body to provide a lead-rich atmosphere. First, the binder is removed at 650°C for 8 hours, and then the temperature is increased to 1250°C at a heating rate of 5°C / min and sintered for 2 hours to obtain Mn-doped PIN-PSN-PT ceramics.

[0049] (5) The obtained Mn-doped PIN-PSN-PT ceramic was polished into a disc with a thickness of 0.8 mm, and a conductive silver paste was brushed on the surface. Then, it was placed on an alumina ceramic plate and silver was calcined at 600°C for 20 min. After that, it was subjected to high-temperature polarization treatment. It was polarized for 20 min under a DC electric field of 20 kV / cm and the polarization temperature was 120°C. After standing for two weeks for aging, a Mn-doped PIN-PSN-PT hard piezoelectric ceramic material was obtained.

[0050] The preparation method of the lead compensation sheet in step (4) is: first weigh PbO and ZrO2 according to a stoichiometric ratio of 1:1, mix them by ball milling, dry the discharged materials, and then directly dry press them under a uniaxial pressure of 10 MPa.

[0051] The performance test results show that the hard piezoelectric ceramic material prepared in this embodiment is a pure ABO3 perovskite phase without pyrochlore phase, and its piezoelectric coefficient is 351pC / N, the mechanical quality factor is 2391, the Curie temperature is 300°C, and the dielectric loss is 3.7‰.

[0052] Example 4

[0053] A high Q m , high T c , high d 33 The hard piezoelectric ceramic and the preparation method thereof, the specific steps are:

[0054] (1) Sc(NO3)3, In(OH)3, and Nb2(C2O4)5 are used as raw materials, weighed according to the stoichiometric ratio of ScNbO4 and InNbO4, and placed in a polytetrafluoroethylene ball mill. Anhydrous ethanol is used as the grinding medium and ZrO2 is used as the grinding ball. The ball mill is milled at a speed of 400 r / min for 12 h. The resulting slurry is then placed in an oven and dried at 100°C for 5 h. After drying, the slurry is sieved through a 40-mesh sieve and the sieved powder is placed in an alumina crucible for calcination. ScNbO4 is calcined at 1150°C for 1 h and InNbO4 is calcined at 1050°C for 1 h to obtain ScNbO4 and InNbO4 precursor powders.

[0055] (2) Taking x = 0.395, y = 0.415, z = 0.015, ScNbO4, InNbO4, TiO2, Mn2(C2O4)3, Pb(OH)2 as raw materials, 0.19Pb(In 1 / 2 Nb 1 / 2 )O3-0.395Pb(Sc 1 / 2 Nb 1 / 2 )O3-0.415PbTiO3-0.015Mn with a stoichiometric ratio, put into a polytetrafluoroethylene ball mill, use anhydrous ethanol as the grinding medium and ZrO2 as the grinding balls, and ball mill for 12 hours at a speed of 400r / min. Then, the obtained slurry is placed in an oven and dried at 100°C for 5 hours. After drying, it is sieved through a 40-mesh sieve, and the sieved powder is placed in an alumina crucible and calcined at 800°C for 1 hour to obtain PIN-PSN-PT-Mn powder.

[0056] (3) The obtained PIN-PSN-PT-Mn powder is placed in a ball mill and ball milled again under the same ball milling conditions as in (1) and (2). The obtained slurry is then placed in an oven and baked at 100°C for 5 h. After drying, 2 wt% of polyvinyl alcohol (PVA) is added to the powder as a binder and granulated manually, passed through an 80-mesh sieve, and then 0.8 g of the sieved powder is weighed and dry-pressed at 2 MPa to obtain a ceramic green body. The ceramic green body is in the form of a disc with a diameter of 10 mm and a thickness of 1.8 mm.

[0057] (4) The ceramic green body is placed on an alumina ceramic plate covered with a sealed crucible, and the bottom, sides and top of the green body are filled with PIN-PSN-PT powder of the same mass and composition as the green body. A lead compensation sheet with a mass of 1 / 2 of the green body mass is placed 1 cm away from the green body to provide a lead-rich atmosphere. First, the binder is removed at 550°C for 1h, and then the temperature is increased to 1250°C at a heating rate of 3°C / min and sintered for 4h to obtain Mn-doped PIN-PSN-PT ceramics.

[0058] (5) The obtained Mn-doped PIN-PSN-PT ceramic was polished into a disc with a thickness of 0.8 mm, and a conductive silver paste was brushed on the surface. Then, the disc was placed on an alumina ceramic plate and silver was sintered at 500°C for 30 min. After that, a high-temperature polarization treatment was performed. The disc was polarized for 30 min under a DC electric field of 30 kV / cm and the polarization temperature was 100°C. After standing for one week for aging, a Mn-doped PIN-PSN-PT hard piezoelectric ceramic material was obtained.

[0059] The preparation method of the lead compensation sheet in step (4) is as follows: first weigh PbO and ZrO2 according to a stoichiometric ratio of 1:1, mix them by ball milling, dry the discharged materials, and then directly dry press them under a uniaxial pressure of 2 MPa.

[0060] The performance test results show that the hard piezoelectric ceramic material prepared in this embodiment is a pure ABO3 perovskite phase without pyrochlore phase, and its piezoelectric coefficient is 354pC / N, the mechanical quality factor is 2354, the Curie temperature is 285°C, and the dielectric loss is 4.2‰.

[0061] Example 5

[0062] A high Q m , high T c , high d 33 The hard piezoelectric ceramic and the preparation method thereof, the specific steps are:

[0063] (1) Sc(OH)3, In(NO3)3, and Nb(CH3COO)5 are used as raw materials, weighed according to the stoichiometric ratio of ScNbO4 and InNbO4, and placed in a polytetrafluoroethylene ball mill. Anhydrous ethanol is used as the grinding medium and ZrO2 is used as the grinding ball. The ball mill is milled at a speed of 400 r / min for 12 h. The resulting slurry is then placed in an oven and dried at 100°C for 5 h. After drying, it is sieved through a 40-mesh sieve and the sieved powder is placed in an alumina crucible for calcination. ScNbO4 is calcined at 1200°C for 5 h and InNbO4 is calcined at 1100°C for 5 h to obtain ScNbO4 and InNbO4 precursor powders.

[0064] (2) Taking x = 0.385, y = 0.425, z = 0.02, ScNbO4, InNbO4, TiO2, Mn(CH3COO)3, Pb(NO3)2 as raw materials, 0.19Pb(In 1 / 2 Nb 1 / 2 )O3-0.385Pb(Sc 1 / 2 Nb 1 / 2 )O3-0.425PbTiO3-0.02Mn with a stoichiometric ratio, put into a polytetrafluoroethylene ball mill, use anhydrous ethanol as the grinding medium and ZrO2 as the grinding balls, and ball mill for 12 hours at a speed of 400r / min. Then, the obtained slurry is placed in an oven and baked at 100°C for 5 hours. After drying, it is sieved through a 40-mesh sieve, and the sieved powder is placed in an alumina crucible and calcined at 850°C for 5 hours to obtain PIN-PSN-PT-Mn powder.

[0065] (3) The obtained PIN-PSN-PT-Mn powder is placed in a ball mill and ball milled again under the same ball milling conditions as in (1) and (2). The obtained slurry is then placed in an oven and baked at 100°C for 5 h. After drying, 1 wt% of polyvinyl alcohol (PVA) is added to the powder as a binder and granulated manually, passed through an 80-mesh sieve, and then 0.8 g of the sieved powder is weighed and dry-pressed at 5 MPa to obtain a ceramic green body. The ceramic green body is in the form of a disc with a diameter of 10 mm and a thickness of 1.8 mm.

[0066] (4) The ceramic green body is placed on an alumina ceramic plate covered with a sealed crucible, and the bottom, sides and top of the green body are filled with PIN-PSN-PT powder of the same mass and composition as the green body. A lead compensation sheet with a mass of 1 / 4 of the green body mass is placed 2 cm away from the green body to provide a lead-rich atmosphere. First, the binder is removed at 600°C for 5h, and then the temperature is increased to 1200°C at a heating rate of 4°C / min and sintered for 2h to obtain Mn-doped PIN-PSN-PT ceramics.

[0067] (5) The obtained Mn-doped PIN-PSN-PT ceramic was polished into a disc with a thickness of 0.8 mm, and a conductive silver paste was brushed on the surface. Then, the disc was placed on an alumina ceramic plate and silver was sintered at 550°C for 20 min. After that, a high-temperature polarization treatment was performed under a DC electric field of 20 kV / cm for 20 min at a polarization temperature of 110°C. After standing for one week for aging, a Mn-doped PIN-PSN-PT hard piezoelectric ceramic material was obtained.

[0068] The preparation method of the lead compensation sheet in step (4) is: first weigh PbO and ZrO2 according to a stoichiometric ratio of 1:1, mix them by ball milling, dry the discharged materials, and then directly dry press them under a uniaxial pressure of 5 MPa.

[0069] The performance test results show that the hard piezoelectric ceramic material prepared in this embodiment is a pure ABO3 perovskite phase without pyrochlore phase, and its piezoelectric coefficient is 381pC / N, the mechanical quality factor is 2201, the Curie temperature is 293°C, and the dielectric loss is 4.3‰.

[0070] Example 6

[0071] A high Q m , high T c , high d 33 The hard piezoelectric ceramic and the preparation method thereof, the specific steps are:

[0072] (1) Sc2(C2O4)3, In2(C2O4)3, and Nb(OH)5 are used as raw materials, weighed according to the stoichiometric ratio of ScNbO4 and InNbO4, and placed in a polytetrafluoroethylene ball mill. Anhydrous ethanol is used as the grinding medium and ZrO2 is used as the grinding ball. The ball mill is milled at a speed of 400 r / min for 12 h. The resulting slurry is then placed in an oven and dried at 100°C for 5 h. After drying, the slurry is sieved through a 40-mesh sieve and the sieved powder is placed in an alumina crucible for calcination. ScNbO4 is calcined at 1250°C for 8 h and InNbO4 is calcined at 1150°C for 8 h to obtain ScNbO4 and InNbO4 precursor powders.

[0073] (2) Taking x = 0.385, y = 0.425, z = 0.025, ScNbO4, InNbO4, TiO2, Mn(OH)4, PbC2O4 as raw materials, 0.19Pb(In 1 / 2 Nb 1 / 2 )O3-0.385Pb(Sc 1 / 2 Nb 1 / 2 )O3-0.425PbTiO3-0.025Mn with a stoichiometric ratio, put it into a polytetrafluoroethylene ball mill, use anhydrous ethanol as the grinding medium and ZrO2 as the grinding balls, and ball mill it at a speed of 400r / min for 12h, then put the obtained slurry into an oven and bake it at 100℃ for 5h, then pass it through a 40-mesh sieve after drying, put the sieved powder into an alumina crucible and calcine it at 900℃ for 8h to obtain PIN-PSN-PT-Mn powder.

[0074] (3) The obtained PIN-PSN-PT-Mn powder is placed in a ball mill and ball milled again under the same ball milling conditions as in (1) and (2). The obtained slurry is then placed in an oven and baked at 100°C for 5 h. After drying, 2 wt% of polyvinyl alcohol (PVA) is added to the powder as a binder and granulated manually, passed through an 80-mesh sieve, and then 0.8 g of the sieved powder is weighed and dry-pressed at 10 MPa to obtain a ceramic green body. The ceramic green body is in the form of a disc with a diameter of 10 mm and a thickness of 1.8 mm.

[0075] (4) The ceramic green body is placed on an alumina ceramic plate covered with a sealed crucible, and the bottom, sides and top of the green body are filled with PIN-PSN-PT powder of the same mass and composition as the green body. A lead compensation sheet with a mass of 1 / 2 of the green body mass is placed 3 cm away from the green body to provide a lead-rich atmosphere. First, the binder is removed at 650°C for 8 hours, and then the temperature is increased to 1200°C at a heating rate of 5°C / min and sintered for 4 hours to obtain Mn-doped PIN-PSN-PT ceramics.

[0076] (5) The obtained Mn-doped PIN-PSN-PT ceramic was polished into a disc with a thickness of 0.8 mm, and a conductive silver paste was brushed on the surface. Then, it was placed on an alumina ceramic plate and silver was sintered at 600°C for 30 min. After that, it was subjected to high-temperature polarization treatment. It was polarized for 30 min under a DC electric field of 30 kV / cm and the polarization temperature was 120°C. After standing for two weeks for aging, a Mn-doped PIN-PSN-PT hard piezoelectric ceramic material was obtained.

[0077] The preparation method of the lead compensation sheet in step (4) is: first weigh PbO and ZrO2 according to a stoichiometric ratio of 1:1, mix them by ball milling, dry the discharged materials, and then directly dry press them under a uniaxial pressure of 10 MPa.

[0078] The performance test results show that the hard piezoelectric ceramic material prepared in this embodiment is a pure ABO3 perovskite phase without pyrochlore phase, and its piezoelectric coefficient is 377pC / N, the mechanical quality factor is 2109, the Curie temperature is 300°C, and the dielectric loss is 2.69‰.

[0079] refer to Figure 1 , XRD diffraction patterns of ceramic materials prepared in Examples 1, 2, and 3 of the present invention, all three ceramics are pure perovskite structures without pyrochlore phase. Table 1 compares the performance of the hard piezoelectric ceramics prepared in Examples 1-6 of the present invention with commercial PZT system hard piezoelectric ceramics (Comparative Example 1) and Yb-doped PZT-PSM system hard piezoelectric ceramics (Comparative Example 2). The results show that compared with traditional PZT system piezoelectric ceramics, the piezoelectric coefficient, mechanical quality factor, and Curie temperature of the ceramics prepared in the present invention are greatly improved. Reference Figure 2 , the scanning electron microscope spectrum of the ceramic material prepared in Example 1 of the present invention, the ceramic has high density and low porosity, reference Figure 3 , the dielectric constant and dielectric loss of the ceramic material prepared in Example 2 of the present invention vary with temperature, the Curie temperature of the ceramic is 300°C, and there is no rhombohedral-tetragonal ferroelectric phase transition above room temperature; reference Figure 4 The electrostrain curves of the ceramic materials prepared in Examples 1, 2, and 3 of the present invention show that the strain and the electric field are approximately linearly related, indicating that the strain hysteresis of the ceramic is relatively low.

[0080] Table 1

[0081]

Claims

1. A Mn-doped PIN-PSN-PT hard piezoelectric ceramic, characterized in that: The Mn-doped hard piezoelectric ceramic material has the following general composition formula: (1-xy)Pb(In 1 / 2 Nb 1 / 2 )O3-xPb(Sc 1 / 2 Nb 1 / 2 )O3-yPbTiO3-zMn, wherein 0.385≤x≤0.405, 0.405≤y≤0.425, 0.015≤z≤0.025; Mn-doped PIN-PSN-PT hard piezoelectric ceramics are prepared by a B-site cation precursor method combined with a high-temperature solid phase reaction synthesis method, specifically comprising the following steps: Step 1, according to the chemical formula (1-xy)Pb(In 1 / 2 Nb 1 / 2 )O3-xPb(Sc 1 / 2 Nb 1 / 2 )O3-yPbTiO3-zMn stoichiometric ratio ScNbO4 precursor powder, InNbO4 precursor powder, TiO2, manganese source and lead source were weighed, ball milled and mixed evenly and dried, and then calcined at 800-900℃ for 1-8h to obtain Pb(In 1 / 2 Nb 1 / 2 )O3-Pb(Sc 1 / 2 Nb 1 / 2 )O3-PbTiO3-Mn powder; the preparation of ScNbO4 and InNbO4 precursor powders comprises the following steps: weighing a scandium source, an indium source and a niobium source according to the stoichiometric ratio of the chemical formula ScNbO4 and InNbO4, respectively, mixing them uniformly by ball milling, drying the uniformly mixed raw materials, and calcining them at 1150-1250° C. and 1050-1150° C. for 1-8 hours, respectively, to obtain ScNbO4 precursor powder and InNbO4 precursor powder; Step 2: Pb(In 1 / 2 Nb 1 / 2 )O3-Pb(Sc 1 / 2 Nb 1 / 2 )O3-PbTiO3-Mn powder is put into a ball mill, and after being evenly mixed and dried, 1wt%-2wt% of polyvinyl alcohol is added as a binder, granulated and sieved, and dry-pressed under a pressure of 2-10MPa to obtain a ceramic green body; Step 3, placing the ceramic green body in PIN-PSN-PT powder, placing a lead compensation sheet at a distance of 1-3 cm from the green body, and covering the crucible to provide a lead-rich atmosphere; after heating to debind and sintering, the Mn-doped PIN-PSN-PT hard piezoelectric ceramic is obtained; first, the mixture is kept at 550°C-650°C for 1-8 hours for debinding, and then the mixture is heated to 1200-1300°C at a heating rate of 3-5°C / min, and the mixture is kept at this temperature for 2-4 hours for sintering.

2. The Mn-doped PIN-PSN-PT hard piezoelectric ceramic according to claim 1, characterized in that: It is a pure ABO3 perovskite structure without pyrochlore phase.

3. The Mn-doped PIN-PSN-PT hard piezoelectric ceramic according to claim 1, characterized in that: The scandium source, indium source, niobium source and lead source are Sc 3+ 、In 3+ , Nb 5+ , Pb 2+ The corresponding carbonate, acetate, hydroxide, nitrate, oxalate or oxide, the manganese source can be Mn 2+ , Mn 3+ or Mn 4+ The corresponding carbonates, acetates, hydroxides, nitrates, oxalates or oxides.

4. The Mn-doped PIN-PSN-PT hard piezoelectric ceramic according to claim 1, characterized in that: The preparation method of the lead compensation sheet in step 3 is: first weigh PbO and ZrO2 according to a stoichiometric ratio of 1:1, mix them by ball milling, dry the discharged materials and directly dry-press them under a pressure of 2-10MPa to obtain the lead compensation sheet.

5. The Mn-doped PIN-PSN-PT hard piezoelectric ceramic according to claim 1, characterized in that: In step 3, the ceramic green body is placed in PIN-PSN-PT powder of the same mass and composition as the green body, and the mass of the lead compensation sheet is 1 / 4-1 / 2 of the mass of the green body.

Citation Information

Patent Citations

  • Lead-based (001) C texture piezoelectric ceramic material with high Tr-t and high Tc, and preparation method thereof

    CN110981480A

  • High-piezoelectricity low-loss donor-acceptor co-doped piezoelectric ceramic as well as preparation method and application thereof

    CN113292340A

  • Preparation method of hard piezoelectric ceramic material

    CN114249592A

  • Preparation method of high-performance piezoelectric ceramic

    CN115340377A

  • Quaternary relaxation piezoelectric single crystal material and growing method thereof