A method for removing cold steel from a vacuum chamber of an RH furnace

By adopting carbon deoxygenation method in the RH furnace and using carbon oxygen reaction to remove cold steel in the vacuum chamber, the problems of long time to remove cold steel, large consumption and serious pollution in the prior art are solved, and rapid and pollution-free cold steel removal is achieved. Improves production efficiency and environmental protection.

CN116716454BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310584261.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-03
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

When removing cold steel in the RH furnace vacuum chamber, the prior art has a long operating time and high gas and oxygen consumption, accompanied by smoke pollution, which affects production capacity release and environmental protection.

Method used

Carbon deoxygenation method is used to generate CO gas through violent reaction between carbon and oxygen, and the cold steel in the vacuum chamber is washed away to reduce flue gas pollution caused by oxygen purge. Specific steps include controlling the end point temperature and oxygen value of the converter, increasing the flow of argon gas, adding carbon enhancers in batches, promoting carbon-oxygen reactions, and quickly removing cold steel.

Benefits of technology

It realizes rapid and effective removal of cold steel, reduces flue gas pollution, improves degassing effect, extends the service life of the vacuum chamber, improves the RH operating rate, avoids unqualified molten steel composition, and reduces economic losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116716454B_ABST
    Figure CN116716454B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for removing cold steel in a vacuum chamber by carbon deoxidation using RH, comprising the following steps: 1) converter control: low silicon aluminum steel is boiled out, the converter terminal temperature is 1670-1690°C, and the converter terminal oxygen value is controlled at 450-800ppm; 2) RH control: the molten steel inlet temperature satisfies: the molten steel inlet temperature - the molten steel outlet temperature ≥30°C; the vacuum degree is controlled at 10-15kPa, and the argon gas flow rate is controlled at 100-110Nm 3 / h; add carburizer in batches; increase the argon flow rate to 110~120Nm 3 / h, cancel pressure control, start all vacuum pumps; perform oxygen sedation, and adjust C composition. The advantages are: by using carbon deoxidation to remove RH cold steel when processing boiling steel in RH production, a large amount of CO gas is produced by the violent reaction of carbon and oxygen to violently flush the vacuum chamber, thereby achieving rapid and effective removal of RH cold steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of steelmaking production, and in particular relates to a method for removing cold steel in a vacuum chamber of an RH furnace when RH is used to treat molten steel. Background Art

[0002] When the RH furnace processes molten steel, some droplets generated by splashing will accumulate in the vacuum chamber through multiple furnaces to form cold steel. Figure 1 . The cold steel in the vacuum chamber will not only affect the vacuum degassing effect, but also deteriorate the quality of the molten steel after RH furnace refining. Moreover, when there is too much cold steel, it is easy to add alloy to the cold steel when adding alloy, resulting in unqualified molten steel composition. If the cold steel in the vacuum chamber of the RH furnace is to be removed, an oxygen gun is usually used to blow oxygen and bake the vacuum chamber, and the cold steel operation is carried out for at least one hour; for example, patent application number: CN201510036630.9 discloses a method for removing cold steel in the middle and bottom grooves of the RH vacuum chamber. Before the RH vacuum chamber is put on line to process molten steel, an oxygen gun with low gun position and high flow rate gas is used to bake the lower part of the vacuum chamber to preheat the furnace bottom; in the later stage of the RH vacuum chamber, boiling steel molten steel is used to enter the station to flush the vacuum chamber, and then the slag is scraped to clean the residue on the outer wall of the insertion tube; when the vacuum chamber is offline, it is purged with an oxygen gun to finally remove the cold steel in the middle and bottom grooves; this operation takes a long time to cool the steel, consumes a lot of gas and oxygen, and is accompanied by a large amount of smoke and dust, which not only affects the release of production capacity, but also increases production costs and puts pressure on environmental protection. Summary of the invention

[0003] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a method for removing cold steel in the vacuum chamber of an RH furnace. When treating boiling steel, a carbon deoxidation method is adopted, and a large amount of CO gas is produced by the violent reaction between carbon and oxygen to flush the cold steel, thereby reducing the flue gas pollution caused by oxygen purging of the cold steel.

[0004] To achieve the above object, the present invention is implemented through the following technical solutions:

[0005] A method for removing cold steel in a vacuum chamber by carbon deoxidation in RH comprises the following steps:

[0006] 1) Converter control: Low silicon aluminum steel is tapped by boiling, the converter endpoint temperature is controlled at 1670-1690°C, and the converter endpoint oxygen value is controlled at 450-800ppm;

[0007] 2)RH control:

[0008] a. The temperature of molten steel entering the station meets the following requirements:

[0009] Molten steel inlet temperature - molten steel outlet temperature ≥ 30℃;

[0010] b After the vacuum pump is started, turn on the pressure control, control the vacuum degree at 10-15kPa, and increase the argon flow rate to 100-110Nm3 / h;

[0011] c. 1.5 to 2 minutes after the vacuum pump is started, add the carburizer in batches; the amount of carburizer added in each batch shall not exceed 0.15 kg / ton of steel, and the batch interval time shall be 2 ± 1 min;

[0012] d. Calculate excess oxygen based on the oxygen value at the station and the carbon content at the argon station:

[0013] Excess oxygen = fixed oxygen value - (initial carbon content - 70) × δ - 150 (1)

[0014] In formula (1), the unit of excess oxygen is ppm; the unit of fixed oxygen value is ppm; the unit of initial carbon content is ppm; δ is the decarburization oxygen coefficient;

[0015] eAfter the last batch of carburizer is added, increase the argon flow rate to 110-120 Nm 3 / h, cancel pressure control, start all vacuum pumps, speed up molten steel circulation, promote carbon-oxygen reaction, rinse cold steel in vacuum chamber; carry out oxygen sedation 9 to 10 minutes after the vacuum pump is started; adjust the C component according to the carbon mass content at the decarburization endpoint to 0.007% to 0.01%.

[0016] The value of the decarburization oxygen coefficient δ is related to the initial carbon content:

[0017] When the initial carbon content is ≤300ppm, the oxygen coefficient for decarburization is δ=0.75;

[0018] When 300ppm<initial carbon content≤500ppm, decarburization oxygen coefficient δ=0.70

[0019] When 500ppm<initial carbon content≤600ppm, decarburization oxygen coefficient δ=0.65;

[0020] When the initial carbon content is greater than 600 ppm, the oxygen coefficient for decarburization is δ=0.80.

[0021] The total amount of the recarburizer added is related to the excess oxygen:

[0022] When excess oxygen is less than 200ppm, the amount of carburizer added = excess oxygen × 0.00173; the unit of the amount of carburizer added is kg / ton of steel, and 0.00173 is the empirical coefficient;

[0023] When the excess oxygen is ≥200ppm, the maximum amount of recarburizer added is 0.7kg / ton of steel.

[0024] Repeat steps 1) to 2) for 2 to 4 cycles until the two insertion tubes in the vacuum chamber can be fully observed after rinsing.

[0025] The low silicon aluminum steel comprises, by mass percentage: 0.01%≤C≤0.1%, Si≤0.05%.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention removes RH cold steel by using a carbon deoxidation method when processing boiling steel in RH production, and utilizes the violent reaction between carbon and oxygen to generate a large amount of CO gas to violently flush the vacuum chamber, thereby achieving rapid and effective removal of RH cold steel and reducing flue gas pollution caused by the method of using oxygen to purge cold steel. After the cold steel is removed, the degassing effect can be improved, the service life of the vacuum chamber can be extended, the RH operating rate can be increased, and the incompatibility of components and excessive inclusions caused by a small amount of cold steel melting into molten steel when smelting special steel grades can be avoided. The method of the present invention removes RH cold steel without pollution, provides assistance for production and component stability, and reduces a large amount of economic losses in steel mills. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a schematic diagram of a vacuum chamber in which RH cold steel is stacked.

[0029] Figure 2 It is a schematic diagram of the vacuum chamber after the cold steel is flushed away by the method of the present invention.

[0030] In the figure: 1-cold steel 2-inside of vacuum chamber. DETAILED DESCRIPTION

[0031] The present invention is described in detail below in conjunction with the accompanying drawings, but it should be noted that the implementation of the present invention is not limited to the following embodiments.

[0032] A method for removing cold steel in a vacuum chamber by carbon deoxidation in RH comprises the following steps:

[0033] 1) Converter control: Low silicon aluminum steel is tapped by boiling, the converter endpoint temperature is controlled at 1670-1690℃, and the converter endpoint oxygen value is controlled at 450-800ppm; the converter endpoint temperature is controlled to prevent the molten steel from continuing to form cold steel after the cold steel is rinsed off in the RH vacuum chamber, and to prevent the molten steel from being polluted by a large temperature rise due to a large drop in temperature after the cold steel is rinsed off; the high oxygen value is controlled to make the carbon-oxygen reaction of the molten steel more sufficient and more intense during the RH vacuum treatment.

[0034] Low silicon aluminum steel includes, by mass percentage: 0.01%≤C≤0.1%, Si≤0.05%.

[0035] 2)RH control:

[0036] a. The temperature of molten steel entering the station meets the following requirements:

[0037] Molten steel inlet temperature - molten steel outlet temperature ≥ 30℃.

[0038] b After the vacuum pump is started, turn on the pressure control, control the vacuum degree at 10-15kPa, and increase the argon flow rate to 100-110Nm 3 / h. The high vacuum degree and low argon flow rate in the early stage were used to avoid excessive splashing caused by excessive carbon-oxygen reaction in the early stage, which instead sprayed cold steel on the hot top cover of the vacuum chamber;

[0039] c. 1.5 to 2 minutes after the vacuum pump is started, add the carburizer in batches; the amount of carburizer added in each batch shall not exceed 0.15 kg / ton of steel, and the batch interval time shall be 2 ± 1 minutes. The carburizer can be 90 carburizer or 95 carburizer.

[0040] The total amount of recarburizer added is related to the excess oxygen:

[0041] When excess oxygen is less than 200ppm, the amount of carburizer added = excess oxygen × 0.00173; the unit of the amount of carburizer added is kg / ton steel, 0.00173 is the empirical coefficient, the unit is kg / (ton steel * ppm);

[0042] Taking a 260-ton RH furnace as an example, when excess oxygen is less than 200 ppm, the amount of recarburizer added = excess oxygen × 0.45; the unit of the amount of recarburizer added is kg, and 0.45 is the empirical coefficient, the unit is kg / ppm.

[0043] When the excess oxygen is ≥200ppm, the maximum amount of recarburizer added is 0.7kg / ton of steel.

[0044] d. Calculate excess oxygen based on the oxygen value at the station and the carbon content at the argon station:

[0045] Excess oxygen = fixed oxygen value - (initial carbon content - 70) × δ - 150 (1)

[0046] In formula (1), the unit of excess oxygen is ppm; the unit of fixed oxygen value is ppm; the unit of initial carbon content is ppm; δ is the decarburization oxygen coefficient;

[0047] The value of the decarburization oxygen coefficient δ is related to the initial carbon content:

[0048] When the initial carbon content is ≤300ppm, the oxygen coefficient for decarburization is δ=0.75;

[0049] When 300ppm<initial carbon content≤500ppm, decarburization oxygen coefficient δ=0.70

[0050] When 500ppm<initial carbon content≤600ppm, decarburization oxygen coefficient δ=0.65;

[0051] When the initial carbon content is greater than 600 ppm, the oxygen coefficient for decarburization is δ=0.80.

[0052] eAfter the last batch of carburizer is added, increase the argon flow rate to 110-120 Nm 3 / h, cancel the pressure control, start all vacuum pumps, maintain rapid molten steel circulation when the carbon-oxygen reaction is no longer too intense, promote the carbon-oxygen reaction, and continue to rinse the cold steel in the vacuum chamber. Oxygen sedation is performed 9 to 10 minutes after the vacuum pump is started; the carbon mass content at the decarburization endpoint is adjusted to 0.007% to 0.01% for the C component.

[0053] Example 1

[0054] The method of removing cold steel from the vacuum chamber of the RH furnace, the RH furnace is a 260-ton furnace, the process route is: converter → argon station → RH → casting machine, smelting steel grade SPHC, including the following steps:

[0055] 1) The final converter temperature is 1681°C and the final oxygen value is 621ppm;

[0056] 2) RH inlet temperature 1624°C, inlet oxygen value 506ppm, initial carbon content 381ppm, and outlet temperature 1589°C;

[0057] 3) After the vacuum pump is started, select pressure control, adjust the pressure to 15kPa, and increase the gas flow rate to 100Nm 3 / h;

[0058] 4) Calculate the excess oxygen according to formula (1) to obtain an excess oxygen value of 138.3 ppm, and the total amount of recarburizer added is about 62 kg.

[0059] 5) The first batch of carburizer (38 kg) was added after 102 seconds of vacuum pump startup, and the second batch of carburizer (24 kg) was added after 185 seconds of vacuum pump startup;

[0060] 6) After the second batch of carburizer is added, the lifting gas is adjusted to 118Nm 3 / h, and cancel pressure control at the same time;

[0061] 7) Start the vacuum pump for 9 minutes and 40 seconds to stabilize oxygen, add aluminum wire segments for deoxidation, add other alloys, measure the temperature at 1587℃, move out, and put on the casting machine;

[0062] 8) Continue to rinse 2-3 furnaces and repeat steps 1-7 until the two insertion tubes in the vacuum chamber can be fully observed after rinsing. Figure 2 , indicating that most of the cold steel in the vacuum chamber has been removed. Figure 2 It can be seen that the interior of the vacuum chamber 2 can be clearly seen after the cold steel is basically removed.

[0063] Example 2

[0064] The method of removing cold steel from the vacuum chamber of the RH furnace, the RH furnace is a 260-ton furnace, the process route is: converter → argon station → RH → casting machine, smelting steel grade SPCC, including the following steps:

[0065] 1) The final converter temperature is 1684°C and the final oxygen value is 583ppm;

[0066] 2) RH inlet temperature 1625°C, inlet oxygen value 496ppm, initial carbon content 423ppm, and outlet temperature 1588°C;

[0067] 3) After the vacuum pump is started, select pressure control, adjust the pressure to 15kPa, and increase the gas flow rate to 104Nm 3 / h;

[0068] 4) Calculate the excess oxygen according to formula (1) to obtain an excess oxygen value of 98.9 ppm, and the total amount of recarburizer added is about 45 kg. The recarburizer can be 90 recarburizer or 95 recarburizer.

[0069] 5) The first batch of carburizer (25 kg) was added after 107 seconds of vacuum pump startup, and the second batch of carburizer (20 kg) was added after 188 seconds of vacuum pump startup;

[0070] 6) After the second batch of carburant is added, the lifting gas is adjusted to 119Nm 3 / h, and cancel pressure control at the same time;

[0071] 7) The vacuum pump is started for 9 minutes and 45 seconds to stabilize oxygen, aluminum wire is added for deoxidation, other alloys are added, the temperature is measured at 1589°C, the machine is moved out, and the casting is started;

[0072] 8) Continue rinsing 2-3 furnaces and repeat steps 1-7 to remove most of the cold steel in the vacuum chamber.

[0073] Example 3

[0074] The method for removing cold steel from the vacuum chamber of the RH furnace, the RH furnace is a 260-ton furnace, the process route is: converter → argon station → RH → casting machine, smelting steel grade SAE1005, including the following steps:

[0075] 1) The final converter temperature is 1686°C and the final oxygen value is 782ppm;

[0076] 2) RH inlet temperature 1630℃, inlet oxygen value 696ppm, initial carbon content 324ppm, and outlet temperature 1590℃;

[0077] 3) After the vacuum pump is started, select pressure control, adjust the pressure to 14kPa, and increase the gas flow rate to 102Nm 3 / h;

[0078] 4) Calculate the excess oxygen according to formula (1) to obtain an excess oxygen value of 368.2 ppm, and the total amount of recarburizer added is about 166 kg.

[0079] 5) Add the first batch of carburizer 39 kg at 94 s after the vacuum pump is started, add the second batch of carburizer 39 kg at 157 s after the vacuum pump is started, add the third batch of carburizer 39 kg at 218 s after the vacuum pump is started, add the fourth batch of carburizer 38 kg at 280 s after the vacuum pump is started, and add the fourth batch of carburizer 11 kg at 345 s after the vacuum pump is started;

[0080] 6) After the fourth batch of carburant is added, the lifting gas is adjusted to 116Nm 3 / h, and cancel pressure control at the same time;

[0081] 7) The vacuum pump is started for 9 minutes and 55 seconds to stabilize oxygen, add aluminum wire segments for deoxidation, add other alloys, measure the temperature at 1590℃, move out, and put on the casting machine;

[0082] 8) Continue to rinse 2-3 furnaces and repeat steps 1-7 until the two insertion tubes in the vacuum chamber can be fully observed, indicating that most of the cold steel in the vacuum chamber has been removed.

Claims

1. A method for removing cold steel in a vacuum chamber by carbon deoxidation in RH, characterized in that: The following steps are involved: 1) Converter control: Low silicon aluminum steel is tapped by boiling, the converter endpoint temperature is controlled at 1670-1690°C, and the converter endpoint oxygen value is controlled at 450-800ppm; 2)RH control: a. The temperature of molten steel entering the station meets the following requirements: Molten steel inlet temperature - molten steel outlet temperature ≥ 30℃; b After the vacuum pump is started, turn on the pressure control, control the vacuum degree at 10-15kPa, and increase the argon flow rate to 100-110Nm 3 / h; c. 1.5 to 2 minutes after the vacuum pump is started, add the carburizer in batches; the amount of carburizer added in each batch shall not exceed 0.15 kg / ton of steel, and the batch interval time shall be 2 ± 1 min; d. Calculate excess oxygen based on the oxygen value at the station and the carbon content at the argon station: Excess oxygen = fixed oxygen value - (initial carbon content - 70) × δ - 150 (1) In formula (1), the unit of excess oxygen is ppm; the unit of fixed oxygen value is ppm; the unit of initial carbon content is ppm; δ is the oxygen coefficient for decarburization; eAfter the last batch of carburizer is added, increase the argon flow rate to 110-120 Nm 3 / h, cancel pressure control, start all vacuum pumps, speed up molten steel circulation, promote carbon-oxygen reaction, rinse cold steel in vacuum chamber; carry out oxygen sedation 9 to 10 minutes after the vacuum pump is started; adjust the C component according to the carbon mass content at the decarburization endpoint to 0.007% to 0.01%.

2. A method for removing cold steel in a vacuum chamber by carbon deoxidation in RH according to claim 1, characterized in that: The value of the decarburization oxygen coefficient δ is related to the initial carbon content: When the initial carbon content is ≤300ppm, the oxygen coefficient for decarburization is δ=0.75; When 300ppm<initial carbon content≤500ppm, decarburization oxygen coefficient δ=0.70 When 500ppm<initial carbon content≤600ppm, decarburization oxygen coefficient δ=0.65; When the initial carbon content is greater than 600 ppm, the oxygen coefficient for decarburization is δ=0.

80.

3. The method for removing cold steel in a vacuum chamber by carbon deoxidation in RH according to claim 1, characterized in that: The total amount of the recarburizer added is related to the excess oxygen: When excess oxygen is less than 200ppm, the amount of carburizer added = excess oxygen × 0.00173; the unit of the amount of carburizer added is kg / ton of steel, and 0.00173 is the empirical coefficient; When the excess oxygen is ≥200ppm, the maximum amount of recarburizer added is 0.7kg / ton of steel.

4. The method of removing cold steel in a vacuum chamber by carbon deoxidation in RH according to claim 1, characterized in that: Repeat steps 1) to 2) for 2 to 4 cycles until the two insertion tubes in the vacuum chamber can be fully observed after rinsing.

5. The method of removing cold steel in a vacuum chamber by carbon deoxidation in RH according to claim 1, characterized in that: The low silicon aluminum steel comprises, by mass percentage: 0.01%≤C≤0.1%, Si≤0.05%.