A kind of hydrocarbon resistant plug valve sealing grease and preparation method thereof
By using a plug valve sealing grease composition with polyether base oil and high-purity inorganic thickener, the problem of dilution and dispersion loss of traditional mineral oil grease by hydrocarbon media is solved, achieving long service life and high-efficiency sealing performance of plug valves.
Patent Information
- Application Number
- CN202310435897.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-22
AI Technical Summary
Existing plug valve sealing greases are prone to chemical reactions when in contact with hydrocarbon media, leading to viscosity loss, dispersion and leakage, insufficient sealing and pressure resistance, and in severe cases, sealing leakage and accidents.
A hydrocarbon-resistant plug valve sealing grease composition is formed by replacing traditional mineral oil with polyether base oil, and combining high-purity inorganic mica powder and silica thickener, along with adhesives, antioxidants, rust inhibitors, extreme pressure agents and polymerization inhibitors, thus improving its adhesion, sealing and pressure resistance.
It effectively extends the service life and grease change cycle of the plug valve, improves sealing performance and pressure resistance, prevents grease dilution and dispersion, and ensures the safe and stable operation of the equipment.
Smart Images

Figure CN116731769B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lubricating grease, and in particular relates to a composition and a preparation method of a plug valve sealing lubricating grease for transporting hydrocarbons. Background Art
[0002] The valve is one of the control components of the fluid delivery system. As a type of valve, the plug valve is a valve that uses a conical or cylindrical "plug" to stop or start the flow. It is widely used in oilfield mining, transportation and refining equipment, as well as petrochemical, natural gas and liquefied petroleum gas industries. The working pressure can reach 150MPa, the maximum working temperature can reach above 300℃, and the maximum diameter can reach 600mm. In order to reduce the friction between the valve body and the plug sealing surface, the valve seat is generally lubricated with sealing grease. The sealing grease has the properties of non-solidification, non-dispersion, non-dissolution and good pressure resistance. It is one of the key measures to reduce the wear of the valve sealing surface and increase the service life of the valve. The existing valve sealing grease is composed of mineral oil, refined mineral oil or high-viscosity silicone oil thickened with inorganic thickener and added with structural stabilizer, antioxidant, corrosion-resistant and water-resistant agent. It has good sealing, waterproof and anti-creeping properties, does not corrode metal, and has good compatibility with rubber. The service life and replacement of sealing grease are usually determined according to the conveying medium and the number of times the valve is switched. Reasonable valve sealing grease should be selected according to different conveying media, especially when the conveying medium is hydrocarbon gases such as methane, ethane, propane, ethylene and propylene. The sealing grease in the valve is in full contact with the conveying medium and is prone to chemical reactions. Sealing greases based on mineral oil usually react with hydrocarbon gases to produce substitution reactions, which have a negative impact on the adhesion and sealing properties of the sealing grease. In severe cases, it can cause sealing leakage or even accidents. Summary of the invention
[0003] In order to solve the above problems, the present invention discloses a hydrocarbon-resistant plug valve sealing grease and a preparation method thereof, which uses a polyether base oil to replace the traditional mineral oil. By utilizing the characteristic that this type of base oil has very low solubility in hydrocarbon gases, the plug valve sealing grease can solve the problems of viscosity loss and grease dispersion loss caused by easy dilution and dissolution during use, thereby improving the lubricity and sealing between the valve and the valve body, thereby further improving the problems of insufficient pressure resistance and sealing failure of traditional valve sealing grease, and can effectively extend the working cycle and reduce downtime.
[0004] The technical solution of the present invention is as follows:
[0005] A hydrocarbon-resistant plug valve sealing grease composition is composed of a base oil, a thickener, an adhesive and an additive; the mass percentage of each component is:
[0006] Base oil: its content is 60-85%;
[0007] Thickener: its content is 5-25%;
[0008] Adhesive: Its content is 5-15%;
[0009] Additives: the content is 1-5%;
[0010] Among them, additives include:
[0011] (a) antioxidant, total content of 0.2 to 2.0%;
[0012] (b) rust inhibitor, total content of 0.1 to 5.0%;
[0013] (c) extreme pressure agent, total content of 0.5 to 5.0%;
[0014] (d) Inhibitor, total content is 0.1-0.5%.
[0015] The base oil is a random polymer consisting of butanol, glycol and pentaerythritol as starting points and grafted with ethylene oxide groups (EO) and propylene oxide groups (PO); wherein the mass percentage of polymer 1 containing 50% by weight of ethylene oxide groups and 50% by weight of propylene oxide groups and polymer 2 containing 75% by weight of ethylene oxide groups and 25% by weight of propylene oxide groups is 3:1 to 1:1; the viscosity of the base oil at 40°C is 460-680 mm 2 / s, pour point is lower than -30℃.
[0016] Furthermore, in the above-mentioned hydrocarbon-resistant plug valve sealing grease composition, the thickener is composed of mica powder and fumed and precipitated silica in different proportions; wherein the mass ratio of mica powder to silica is 1:1.5 to 1:3; the mass ratio of fumed silica to precipitated silica is 2:1 to 3:1. The use of high-purity inorganic mica powder and silica materials as thickeners can solve the acid-base reaction and corrosion caused by acidic or alkaline compounds encountered during the use of sealing grease, thereby avoiding the solidification and hardening of the grease.
[0017] Furthermore, in the above-mentioned hydrocarbon-resistant plug valve sealing grease composition, the adhesive is composed of two or more of polyisobutylene, polymethacrylate, polyethylene, polypropylene or ethylene-propylene copolymer, and the content is 5-15%. The use of polyisobutylene, polymethacrylate, polyethylene, polypropylene or ethylene-propylene copolymer can improve the adhesion of the grease, make the grease adhere to the friction pair surface of the "plug" valve, and improve the lubrication and sealing performance of the grease;
[0018] Furthermore, in the above hydrocarbon-resistant plug valve sealing grease composition, the antioxidant is a mixture of 2'6-di-tert-butyl-p-cresol, octyl diphenylamine and diamyl dithiocarbamate, and the content is 0.2-2.0%.
[0019] Furthermore, in the above-mentioned hydrocarbon-resistant plug valve sealing grease composition, the rust inhibitor is a mixture of sorbitol monooleate and barium dinonylnaphthalene sulfonate, and the content is 0.1-5.0%. The use of antioxidants, rust inhibitors and polymerization inhibitors can effectively slow down and prevent the solidification, dispersion and dissolution of the plug valve sealing grease, effectively prevent the polymerization of unsaturated hydrocarbon monomers, and ensure the ductility, adhesion and sealing of the grease.
[0020] Furthermore, in the above-mentioned hydrocarbon-resistant plug valve sealing grease composition, the extreme pressure agent is a mixture of zinc dialkyl dithiophosphate, antimony dialkyl dithiophosphate, Vanlube829, molybdenum thiocarbamate and borate, and the content is 0.5-5.0%. Using the mixture of zinc dialkyl dithiophosphate, antimony dialkyl dithiophosphate, Vanlube829, molybdenum thiocarbamate and borate as the extreme pressure agent, the sulfide molecules, active antimony and molybdenum, and borate can be strongly adsorbed on the metal surface of the friction pair of the "plug" valve, forming a chemical reaction film under high pressure and high temperature conditions, providing excellent extreme pressure performance.
[0021] Furthermore, in the above hydrocarbon-resistant plug valve sealing grease composition, the inhibitor is copper di-n-butyl dithiocarbamate, and its dosage is 0.1 to 0.5% of the total mass of the grease.
[0022] Furthermore, the preparation method of the above-mentioned hydrocarbon-resistant plug valve sealing grease composition comprises the following steps:
[0023] 1) adding a polymer containing 50% by weight of ethylene oxide groups and 50% by weight of propylene oxide groups and a polymer containing 75% by weight of ethylene oxide groups and 25% by weight of propylene oxide groups into a reaction kettle in a specific ratio, mixing and heating to 150° C.;
[0024] 2) Add adhesive, stir for 30 minutes until the adhesive is completely dissolved and then cool to 100°C;
[0025] 3) Slowly add mica powder and inorganic thickeners such as silicon dioxide, and stir for 40 to 100 minutes until all materials are completely dispersed to form a uniform paste;
[0026] 4) Add antioxidant, extreme pressure agent, rust inhibitor and polymerization inhibitor in sequence, and stir for 40 to 100 minutes until all additives are completely dispersed into the above uniform paste;
[0027] 5) When the temperature drops to 40-60°C, grind it three times with a three-roll grinder, take samples and test them before canning.
[0028] Furthermore, the above hydrocarbon-resistant plug valve sealing grease composition or its preparation method is used in equipment for conveying hydrocarbon gases.
[0029] Furthermore, the hydrocarbon gases are methane, ethane, propane, ethylene and propylene. When transporting hydrocarbon gases, the polyether base oil will slow down the substitution reaction with hydrocarbon gases such as ethylene, thereby improving the adhesion and sealing of the sealing grease, and extending the service life of the plug valve and the grease replacement cycle.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The present invention compares base oil, thickener, additive, grease making process and physical and chemical indicators, and combines the fact that hydrocarbon transport media such as methane, ethane, propane, ethylene, propylene, vinyl chloride, etc. easily react chemically with mineral base oil and organic thickener. The present invention provides a hydrocarbon-resistant plug valve sealing grease composition and a preparation method thereof. Polyether base oil is selected as the base oil of the plug valve sealing grease with resistance to hydrocarbons. The low solubility of this type of base oil in hydrocarbon gas can solve the problem of grease loss and sealing failure caused by easy dilution during the use of plug valve sealing grease; high-purity inorganic materials are selected as thickeners. This type of thickener can solve the acid-base reaction, corrosion erosion, high-temperature loss and hardening caused by acid-base compounds during the use of sealing grease; by adding adhesives, antioxidants, rust inhibitors, extreme pressure agents and polymerization inhibitors, a plug valve sealing grease with resistance to hydrocarbons is prepared, which has excellent adhesion, sealing, oxidation resistance, extreme pressure and anti-hydrocarbon reactivity and effectively prevents the polymerization of unsaturated hydrocarbon monomers. It can be used in petrochemical, chemical, natural gas and liquefied petroleum gas industries, and can extend the service life of plug valves and grease replacement cycles. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Comparative diagram of oxidation stability (PDSC) test of plug valve sealing grease obtained in Examples 1-3 and Comparative Examples 1-4;
[0033] Figure 2 Extreme pressure properties of plug valve sealing grease obtained in Examples 1-3 and Comparative Examples 1-4 (four-ball machine method) P D / NTest comparison chart;
[0034] Figure 3A comparison chart of the friction coefficient (25°C, load 100N, frequency 5Hz) of the plug valve sealing grease obtained in Examples 1-3 and Comparative Examples 1-4;
[0035] Figure 4 The aging test (8 cycles) of the plug valve sealing grease obtained in Examples 1-3 and Comparative Examples 1-4 was relatively good;
[0036] Figure 5 Comparison of the leakage-free operation time of the plug valve sealing grease obtained in Examples 1-3 and Comparative Examples 1-4 in ethylene transmission medium equipment. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The reagents or instruments used in the examples of the present invention without indicating the manufacturer are all conventional reagent products that can be obtained through commercial purchase.
[0039] Example 1
[0040] Based on 100% hydrocarbon-resistant plug valve sealing grease, the components and mass percentages are as follows:
[0041] Base oil: content is 65%; it is a random polymer composed of pentaerythritol as the starting point, grafted with ethylene oxide group (EO) and propylene oxide group (PO), composed of polymer 1 containing 50% by weight of ethylene oxide group and 50% by weight of propylene oxide group and polymer 2 containing 75% by weight of ethylene oxide group and 25% by weight of propylene oxide group, the mass ratio of the two is 2:1, and the viscosity at 40°C is 460-680mm 2 / s, pour point is lower than -30℃.
[0042] Thickener: The content is 15%; the thickener is composed of mica powder and fumed and precipitated silica in different proportions; the mass ratio of mica powder to silica is 1:2; the mass ratio of fumed silica to precipitated silica is 2:1;
[0043] Adhesive: content is 15%; composed of polyisobutylene and polymethacrylate, the mass ratio of polyisobutylene to polymethacrylate is 1:2;
[0044] Additives: content is 5%; including:
[0045] (a) an antioxidant having a content of 0.8%, the component being a mixture of 2'6-di-tert-butyl-p-cresol and diamyl dithiocarbamate, with a mass ratio of 1:1;
[0046] (b) a rust inhibitor having a content of 2.5%, the component being a mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705), wherein the preferred mass ratio of the mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705) is 2:1;
[0047] (c) The content of extreme pressure agent is 1.4%, and the components are a mixture of zinc dialkyl dithiophosphate, Vanlube829, and molybdenum thiocarbamate. The mass ratio of the mixture of antimony dialkyl dithiophosphate, Vanlube829, and molybdenum thiocarbamate is 1:2:1;
[0048] (d) The content of the inhibitor is 0.3%, and the component is copper di-n-butyl dithiocarbamate.
[0049] After preparing all the raw materials, the hydrocarbon-resistant plug valve sealing grease, sample number A, can be prepared according to the following preparation method.
[0050] Preparation method: add the base oil into the reaction kettle, mix and heat to 150°C, add the adhesive, stir for 30 minutes until a clear liquid is obtained, and then cool to 100°C; slowly add mica powder, silica and other inorganic thickeners, and stir for 40 to 100 minutes until all materials are completely dispersed to form a uniform paste; add antioxidant, extreme pressure agent, rust inhibitor and polymerization inhibitor in sequence, and stir for 40 to 100 minutes until all additives are completely dispersed into the above uniform paste; when the temperature is reduced to 40 to 60°C, grind three times with a three-roll grinder, take samples for testing, and package after passing the test.
[0051] Example 2
[0052] Based on 100% hydrocarbon-resistant plug valve sealing grease, the components and weight percentages are as follows:
[0053] Base oil: content is 70%; it is a random polymer composed of hexylene glycol as the starting point, grafted with ethylene oxide group (EO) and propylene oxide group (PO), composed of polymer 1 containing 50% by weight of ethylene oxide group and 50% by weight of propylene oxide group and polymer 2 containing 75% by weight of ethylene oxide group and 25% by weight of propylene oxide group, the mass ratio of the two is 2.5:1, and the viscosity at 40°C is 460-680mm 2 / s, pour point is lower than -30℃.
[0054] Thickener: The content is 17%; the thickener is composed of mica powder and fumed and precipitated silica in different proportions. Among them, the mass ratio of mica powder to silica is 1:1.5; the mass ratio of fumed silica to precipitated silica is 2.5:1;
[0055] Adhesive: content is 8%; it is composed of a mixture of polyisobutylene and polypropylene, wherein the mass ratio of polyisobutylene to polypropylene is 2:1;
[0056] Additives: content is 5%; including:
[0057] (a) an antioxidant content of 1.2%, the composition is a mixture of 2'6-di-tert-butyl-p-cresol, octyl diphenylamine and diamyl dithiocarbamate, and the mass ratio of 2'6-di-tert-butyl-p-cresol to octyl diphenylamine is 2:1;
[0058] (b) a rust inhibitor having a content of 2.0%, the component being a mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705), wherein the preferred mass ratio of the mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705) is 1:1;
[0059] (c) an extreme pressure agent having a content of 1.5%, the component being a mixture of antimony dialkyl dithiophosphate and molybdenum thiocarbamate. The mass ratio of the mixture of antimony dialkyl dithiophosphate and molybdenum thiocarbamate is 2:1;
[0060] (d) The content of the inhibitor is 0.3%, and the component is copper di-n-butyl dithiocarbamate.
[0061] After preparing all the raw materials, the hydrocarbon-resistant plug valve sealing grease can be prepared according to the preparation method of Example 1.
[0062] Example 3
[0063] Based on 100% hydrocarbon-resistant plug valve sealing grease, the components and mass percentages are as follows:
[0064] Base oil: content is 75%; it is a random polymer composed of hexylene glycol as the starting point, grafted with ethylene oxide group (EO) and propylene oxide group (PO), composed of polymer 1 containing 50% by weight of ethylene oxide group and 50% by weight of propylene oxide group and polymer 2 containing 75% by weight of ethylene oxide group and 25% by weight of propylene oxide group, the mass ratio of the two is 1:1, and the viscosity at 40°C is 460-680mm 2 / s, pour point is lower than -30℃.
[0065] Thickener: The content is 13%; the thickener is composed of mica powder and fumed and precipitated silica in different proportions. Among them, the mass ratio of mica powder to silica is 1:2.5; the mass ratio of fumed silica to precipitated silica is 3:1;
[0066] Adhesive: content is 7%; it is composed of a mixture of polyisobutylene, polymethacrylate and ethylene-propylene copolymer, with a mass ratio of 2:1:1;
[0067] Additives: content is 5%; including:
[0068] (a) an antioxidant content of 0.5%, the composition is a mixture of 2'6-di-tert-butyl-p-cresol, octyl diphenylamine and diamyl dithiocarbamate, and the mass ratio of 2'6-di-tert-butyl-p-cresol, octyl diphenylamine and diamyl dithiocarbamate is 1:1:1;
[0069] (b) a rust inhibitor having a content of 2.0%, the component being a mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705), wherein the preferred mass ratio of the mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705) is 2:1;
[0070] (c) The content of extreme pressure agent is 2.1%, and the components are zinc dialkyl dithiophosphate, antimony dialkyl dithiophosphate, Vanlube829, molybdenum thiocarbamate and borate, and the mass ratio is 1:1:2:1; (d) The content of inhibitor is 0.4%, and the component is copper di-n-butyl dithiocarbamate.
[0071] Comparative Example 1
[0072] Based on 100% hydrocarbon-resistant plug valve sealing grease, the components and weight percentages are as follows:
[0073] Base oil: content is 70%; base oil is K30 naphthenic oil, mineral oil. (Xinjiang Oilfield K30 naphthenic oil, basic filling mineral oil).
[0074] Thickener: The content is 17%; the thickener is composed of mica powder and fumed and precipitated silica in different proportions. Among them, the mass ratio of mica powder to silica is 1:1.5; the mass ratio of fumed silica to precipitated silica is 2.5:1;
[0075] Adhesive: content is 8%; it is composed of a mixture of polyisobutylene and polypropylene, wherein the mass ratio of polyisobutylene to polypropylene is 2:1;
[0076] Additives: content is 5%; including:
[0077] (a) an antioxidant content of 1.2%, the composition is a mixture of 2'6-di-tert-butyl-p-cresol, octyl diphenylamine and diamyl dithiocarbamate, and the mass ratio of 2'6-di-tert-butyl-p-cresol to octyl diphenylamine is 2:1;
[0078] (b) a rust inhibitor having a content of 2.0%, the component being a mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705), wherein the preferred mass ratio of the mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705) is 1:1;
[0079] (c) an extreme pressure agent having a content of 1.5%, the component being a mixture of antimony dialkyl dithiophosphate and molybdenum thiocarbamate. The mass ratio of the mixture of antimony dialkyl dithiophosphate and molybdenum thiocarbamate is 2:1;
[0080] (d) The content of the inhibitor is 0.3%, and the component is copper di-n-butyl dithiocarbamate.
[0081] Preparation method: Add K30 cycloalkyl oil into a reactor, heat to 150°C, add an adhesive, stir for 30 minutes until a clear liquid is obtained, and then cool to 100°C; slowly add mica powder, silica and other inorganic thickeners, and stir for 40 to 100 minutes until all materials are completely dispersed to form a uniform paste; add antioxidants, extreme pressure agents, rust inhibitors and polymerization inhibitors in sequence, and stir for 40 to 100 minutes until all additives are completely dispersed into the above uniform paste; when the temperature is reduced to 40 to 60°C, grind three times with a three-roll grinder, take samples for testing, and package after passing the test.
[0082] Comparative Example 2
[0083] Based on 100% hydrocarbon-resistant plug valve sealing grease, the components and weight percentages are as follows:
[0084] Base oil: content is 70%; the base oil is obtained by polymerization of butanol and 100% by weight of ethylene oxide.
[0085] Thickener: The content is 17%; the thickener is composed of mica powder and fumed and precipitated silica in different proportions. Among them, the mass ratio of mica powder to silica is 1:1.5; the mass ratio of fumed silica to precipitated silica is 2.5:1;
[0086] Adhesive: content is 8%; it is composed of a mixture of polyisobutylene and polypropylene, wherein the mass ratio of polyisobutylene to polypropylene is 2:1;
[0087] Additives: content is 5%; including:
[0088] (a) an antioxidant content of 1.2%, the composition is a mixture of 2'6-di-tert-butyl-p-cresol, octyl diphenylamine and diamyl dithiocarbamate, and the mass ratio of 2'6-di-tert-butyl-p-cresol to octyl diphenylamine is 2:1;
[0089] (b) a rust inhibitor having a content of 2.0%, the component being a mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705), wherein the preferred mass ratio of the mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705) is 1:1;
[0090] (c) an extreme pressure agent having a content of 1.5%, the component being a mixture of antimony dialkyl dithiophosphate and molybdenum thiocarbamate. The mass ratio of the mixture of antimony dialkyl dithiophosphate and molybdenum thiocarbamate is 2:1;
[0091] (d) The content of the inhibitor is 0.3%, and the component is copper di-n-butyl dithiocarbamate.
[0092] After preparing all the raw materials, the hydrocarbon-resistant plug valve sealing grease can be prepared according to the preparation method of Example 1.
[0093] Comparative Example 3
[0094] Based on 100% hydrocarbon-resistant plug valve sealing grease, the components and weight percentages are as follows:
[0095] Base oil: content is 70%; the base oil is prepared by polymerization of butanol with 75% by weight ethylene oxide groups and 25% by weight propylene oxide groups.
[0096] Thickener: The content is 17%; the thickener is composed of mica powder and fumed and precipitated silica in different proportions. Among them, the mass ratio of mica powder to silica is 1:1.5; the mass ratio of fumed silica to precipitated silica is 2.5:1;
[0097] Adhesive: content is 8%; it is composed of a mixture of polyisobutylene and polypropylene, wherein the mass ratio of polyisobutylene to polypropylene is 2:1;
[0098] Additives: content is 5%; including:
[0099] (a) an antioxidant content of 1.2%, the composition is a mixture of 2'6-di-tert-butyl-p-cresol, octyl diphenylamine and diamyl dithiocarbamate, and the mass ratio of 2'6-di-tert-butyl-p-cresol to octyl diphenylamine is 2:1;
[0100] (b) a rust inhibitor having a content of 2.0%, the component being a mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705), wherein the preferred mass ratio of the mixture of sorbitan monooleate and barium dinonylnaphthalenesulfonate (T705) is 1:1;
[0101] (c) an extreme pressure agent having a content of 1.5%, the component being a mixture of antimony dialkyl dithiophosphate and molybdenum thiocarbamate. The mass ratio of the mixture of antimony dialkyl dithiophosphate and molybdenum thiocarbamate is 2:1;
[0102] (d) The content of the inhibitor is 0.3%, and the component is copper di-n-butyl dithiocarbamate.
[0103] After preparing all the raw materials, the hydrocarbon-resistant plug valve sealing grease can be prepared according to the preparation method of Example 1.
[0104] Comparative Example 4
[0105] A company in the southwest is using a plug valve to seal grease.
[0106] Test Example 1
[0107] The performance of the plug valve sealing grease obtained in Examples 1-3 and Comparative Examples 1-4 was tested, and the results are shown in Tables 1-2 and Attached Figure 1-4 shown.
[0108] Table 1 Analysis and test data comparison
[0109]
[0110] Table 2 Comparison of analysis and test data (continued)
[0111]
[0112] According to Tables 1 and 2 and the attached Figure 1-4It can be seen from the data that Examples 1-3 using polyether base oils to replace traditional mineral oils have excellent performance in corrosion resistance, oxidation stability, extreme pressure performance, high temperature stability, low temperature performance and aging resistance, and have considerable performance improvement compared to Control Examples 1 and 4 using traditional mineral oils. At the same time, Example 2 and Control Example 2 in which butanol is polymerized with a base oil containing only ethylene oxide groups and Control Example 3 in which a base oil is polymerized with butanol containing 75% by weight of ethylene oxide groups and 25% by weight of propylene oxide groups were compared. It has been found that when the composition of the polyether base oil is a random polymer composed of hexylene glycol as the starting point and grafted ethylene oxide groups (EO) and propylene oxide groups (PO), composed of a polymer containing 50% by weight of ethylene oxide groups and 50% by weight of propylene oxide groups and a polymer containing 75% by weight of ethylene oxide groups and 25% by weight of propylene oxide groups, especially when the mass ratio is 2.5:1, the performance can be optimized, and it has excellent non-solidification, non-dispersion, non-solubility, good pressure resistance and sealing properties.
[0113] Test Example 2
[0114] The plug valve sealing grease obtained in the above-mentioned Examples 1-3 and Comparative Examples 1-4 was subjected to an air-tightness test on a PR1 PSL3 PU plug valve conforming to the API standard. After cleaning the valve, the valve was greased by applying sealing grease. The sealing grease was fully adsorbed on the sealing surface by rotating the valve core. The pressure was maintained at 70Mpa-100Mpa and 25°C for 30 minutes. After the pressure was released, the pressure was increased and the pressure was maintained for 50 times. The results are shown in Table 3 below.
[0115] Table 3 Airtightness test
[0116]
[0117] 2. The plug valve sealing grease obtained in Examples 1-3 and Comparative Examples 1-4 was applied to the plug valve of a company in Southwest China. The transport medium was ethylene. The cumulative application time was about 1000 hours (single valve single time 480 hours). During this period, the plug valve worked smoothly, the equipment was in good lubrication condition, met the sealing requirements, and no leakage occurred. The results are shown in Tables 4 and Figure 5 shown.
[0118] Table 4 Application of plug valve sealing grease in ethylene transmission medium equipment.
[0119]
[0120] In summary, the sealing grease composition disclosed in the present invention uses polyether base oil to replace traditional mineral oil. By utilizing the low solubility of this type of base oil in hydrocarbon gas, the problem of grease loss, pressure resistance and sealing failure caused by easy dilution and dissolution during use of the plug valve sealing grease can be solved; high-purity inorganic mica powder and silica material are selected as thickeners, which can solve the problems of acid-base reaction, corrosion erosion, high-temperature loss and solidification hardening caused by acidic or alkaline compounds during use of the sealing grease; the plug valve sealing grease prepared by adding adhesives, antioxidants, rust inhibitors, extreme pressure agents and polymerization inhibitors has excellent non-solidification, non-dispersion, non-solidification, good pressure resistance and sealing properties and anti-hydrocarbon reactivity, and can effectively prevent the polymerization of unsaturated hydrocarbon monomers, thereby ensuring the ductility, adhesion and sealing properties of the grease, and extending the service life of the plug valve and the grease replacement cycle.
[0121] The above are only a few preferred embodiments of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A hydrocarbon-resistant plug valve sealing grease composition, comprising a base oil, a thickener, an adhesive and an additive; characterized in that: The mass percentage of each component is: Base oil: its content is 60-85%; Thickener: its content is 5-25%; Adhesive: Its content is 5-15%; Additives: the content is 1-5%; Among them, additives include: (a) antioxidant, total content of 0.2 to 2.0%; (b) rust inhibitor, total content of 0.1 to 5.0%; (c) extreme pressure agent, total content of 0.5 to 5.0%; (d) polymerization inhibitor, total content of 0.1 to 0.5%; The base oil is a random polymer consisting of hexanediol as a starting point and grafted with ethylene oxide groups EO and propylene oxide groups PO; wherein the mass ratio of polymer 1 containing 50% by weight of ethylene oxide groups and 50% by weight of propylene oxide groups to polymer 2 containing 75% by weight of ethylene oxide groups and 25% by weight of propylene oxide groups is 3:1 to 1:1; the base oil has a viscosity of 460 to 680 mm2 / s at 40°C and a pour point below -30°C; The thickener is composed of a mixture of mica powder and fumed and precipitated silica in different proportions; wherein the mass ratio of mica powder to silica is 1:1.5 to 1:3; and the mass ratio of fumed silica to precipitated silica is 2:1 to 3:
1.
2. The composition according to claim 1, characterized in that The adhesive is composed of two or more of polyisobutylene, polymethacrylate, polyethylene, polypropylene or ethylene-propylene copolymer, with a content of 5-15%.
3. The composition according to claim 1, characterized in that The antioxidant is a mixture of 2'6-di-tert-butyl-p-cresol, octyl diphenylamine and diamyl dithiocarbamate, and the content thereof is 0.2-2.0%.
4. The composition according to claim 1, characterized in that The rust preventive is a mixture of sorbitol monooleate and barium dinonylnaphthalenesulfonate, with a content of 0.1-5.0%.
5. The composition according to claim 1, characterized in that The extreme pressure agent is a mixture of zinc dialkyl dithiophosphate, antimony dialkyl dithiophosphate, Vanlube829, molybdenum thiocarbamate and boric acid ester, and the content thereof is 0.5-5.0%.
6. The composition according to claim 1, characterized in that The polymerization inhibitor is copper di-n-butyl dithiocarbamate, and the dosage thereof is 0.1-0.5% of the total mass of the grease.
7. Use of the composition according to any one of claims 1 to 6 in equipment for conveying hydrocarbon gaseous media.