Alumina ceramic material for thermal quantity sensor
The sintering activity and mechanical properties of alumina ceramic materials are improved through titanium sol coating and multi-stage sintering processes, solving the problem of insufficient thermal shock and achieving efficient application in the aerospace field.
Patent Information
- Application Number
- CN202310628058.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-31
AI Technical Summary
The application of existing thermal sensors in the aerospace field is limited by the insufficient thermal shock and mechanical properties of alumina ceramic materials, and it is difficult to withstand the hot and cold impact of repeated alternating high and low temperatures.
The titanium sol coats alumina powder, nanosilica, graphene oxide, yttrium aluminum garnet pre-made powder and rare earth oxide are used to coat titanium sol and ball milling with the help of sintering additives. Multi-stage sintering process under ammonia atmosphere improves the sintering activity and mechanical properties of alumina ceramic materials.
The thermal shock resistance of alumina ceramic materials was significantly improved. No cracks appeared after 20 alternation of cold and heat. The loss rate of bending strength and fracture toughness was less than 10%, and the mechanical properties and thermal conductivity were improved.
Smart Images

Figure CN116751035B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic materials, in particular to an aluminum oxide ceramic material used for a thermal quantity sensor. Background Art
[0002] There are various types of thermal sensors, including but not limited to heat flow sensors, thermometers, temperature sensors, full radiation pyrometers, etc. As basic tools for measuring heat transfer (heat flux density or heat flux), they are widely used in many fields.
[0003] Thermal sensors in the aerospace field must withstand the test of harsh environments, especially repeated high and low temperature alternations. The plastic shell of a general thermal sensor cannot withstand repeated hot and cold shocks and is prone to cracking. The metal shell is also easy to become brittle due to thermal expansion and contraction. Alumina ceramics have high hardness and good mechanical properties, and a low thermal expansion coefficient. They are often used to make substrates or shells of electronic components. They are ideal materials for making shells of thermal sensors. However, the poor thermal shock resistance of alumina ceramics restricts its use in the aerospace field. Summary of the invention
[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes an alumina ceramic material for thermal quantity sensors.
[0005] The technical solutions adopted are as follows:
[0006] An alumina ceramic material for a thermal quantity sensor comprises the following raw materials in parts by weight:
[0007] 60-80 parts of titanium sol-coated alumina powder, 20-30 parts of nano silicon dioxide, 0.1-0.5 parts of graphene oxide, 10-20 parts of yttrium aluminum garnet prefabricated powder, 2-5 parts of rare earth oxide, and 1-3 parts of sintering aid.
[0008] Furthermore, the alumina ceramic material comprises the following raw materials in parts by weight:
[0009] 75 parts of titanium sol-coated alumina powder, 25 parts of nano-silicon dioxide, 0.25 parts of graphene oxide, 18 parts of yttrium aluminum garnet prefabricated powder, 3 parts of rare earth oxide, and 1 part of sintering aid.
[0010] Furthermore, the preparation method of the titanium sol-coated alumina powder is as follows:
[0011] After uniformly mixing butyl titanate, acetylacetone and the first portion of anhydrous ethanol, the temperature is raised to 60-70°C, and then a mixture consisting of water, concentrated hydrochloric acid and the second portion of anhydrous ethanol is added dropwise, and stirring is continued until the reaction system gradually changes from a colorless transparent liquid to a light yellow-green sol, and the alumina powder is mixed with the sol, ball-milled and dried.
[0012] Furthermore, acetic acid is added during ball milling.
[0013] Furthermore, the preparation method of the yttrium aluminum garnet prefabricated powder is as follows:
[0014] Add yttrium nitrate, aluminum nitrate and citric acid to a mixed solvent consisting of water and anhydrous ethanol, stir and heat to 65-75°C, keep warm for 1-3 hours, then heat to 85-95°C, continue stirring to evaporate the solvent to obtain a gel, transfer the gel to a muffle furnace at 200-250°C for combustion, grind the obtained product, heat to 750-850°C and pre-calcine for 1-2 hours.
[0015] Furthermore, the ratio of the sum of the amounts of yttrium nitrate and aluminum nitrate to the amount of citric acid is 1:0.6-1.
[0016] Furthermore, the rare earth oxide is any one or more combinations of lanthanum oxide, cerium oxide, samarium oxide, neodymium oxide, and yttrium oxide, preferably lanthanum oxide and neodymium oxide, and the weight ratio of the lanthanum oxide to the neodymium oxide is 1-5:1-5.
[0017] Furthermore, the sintering aid includes aluminum trifluoride, vanadium oxide and lithium carbonate, and the weight ratio of the aluminum trifluoride, vanadium oxide and lithium carbonate is 4-8:4-8:0.5-2.
[0018] The present invention also provides a method for preparing an alumina ceramic material:
[0019] Titanium sol-coated alumina powder, nano-silicon dioxide, graphene oxide, yttrium aluminum garnet prefabricated powder, rare earth oxides and sintering aids are mixed and ball-milled to form granules, and then cold isostatically pressed to obtain a green body. The green body is heated to 800-900°C in an ammonia atmosphere, sintered for 3-5 hours, and then the ammonia is replaced by air and heated to 1600-1700°C in a second stage and sintered for 2-4 hours.
[0020] Furthermore, the first stage heating rate is 10-30°C / min, and the second stage heating rate is 1-5°C / min.
[0021] Beneficial effects of the present invention:
[0022] The present invention provides an alumina ceramic material for a thermal quantity sensor. Titanium sol coating of alumina powder can better improve the sintering activity of alumina and reduce the sintering temperature. During the sintering process, the titanium sol peels off from the surface of the alumina powder into fine particles, which can fill the pores inside the ceramic material. Nano-silicon dioxide can obtain a stable silicate liquid phase at high temperature, promote sintering, reduce the sintering temperature, refine the grains, and improve the mechanical properties of the alumina ceramic material. In addition, under the action of a sintering aid, mullite whiskers are generated. The pinning and bridging effects of the mullite whiskers can prevent microcracks from aggregating into critical cracks, thereby The thermal shock resistance of alumina ceramic materials is improved. The addition of yttrium aluminum garnet prefabricated powder can not only play a high-temperature enhancement role, but also improve the mechanical properties of alumina ceramic materials to a certain extent. Graphene oxide can also improve the mechanical properties of alumina ceramic materials, and can act as a reducing agent when sintering in an ammonia atmosphere to promote the formation of metal nitrides with excellent thermal conductivity and improve the thermal shock resistance of alumina ceramic materials. The alumina ceramic material prepared by the present invention has good mechanical properties and good thermal shock resistance. No cracks appear after 20 cycles of hot and cold alternation, and the loss rates of bending strength and fracture toughness are both less than 10%. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of the alumina ceramic material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0024] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0025] Embodiment 1:
[0026] An alumina ceramic material for a thermal quantity sensor comprises the following raw materials in parts by weight:
[0027] Titanium sol coated alumina powder 75 parts, nano silicon dioxide 25 parts, graphene oxide 0.25 parts, yttrium aluminum garnet prefabricated powder 18 parts, lanthanum oxide 2 parts, neodymium oxide 1 part, aluminum trifluoride 0.4 parts, vanadium oxide 0.4 parts, lithium carbonate 0.2 parts.
[0028] The preparation method of titanium sol coated alumina powder is as follows:
[0029] Mix 85g of butyl titanate, 7.5g of acetylacetone and 150ml of anhydrous ethanol, heat to 70°C, and then add a mixture of 18ml of water, 42ml of concentrated hydrochloric acid and 100ml of anhydrous ethanol dropwise. Continue stirring for 2.5h. At this time, the reaction system gradually changes from a colorless transparent liquid to a light yellow-green sol. Stop heating and wait for it to cool naturally. Take 100g of alumina powder and the sol and add them to a ball mill. At the same time, add grinding balls and 1ml of acetic acid to promote gelation. Seal the ball mill and mix and ball mill for 5h. Take out the resulting mixture and dry it at 80°C for 24h.
[0030] The preparation method of yttrium aluminum garnet prefabricated powder is as follows:
[0031] Add 82.5g of yttrium nitrate, 106.5g of aluminum nitrate and 122.9g of citric acid to a mixed solvent consisting of 250ml of water and 250ml of anhydrous ethanol, stir and heat to 75°C, keep warm for 2h, then heat to 95°C, continue stirring to evaporate the solvent for 5h to obtain a gel, transfer the gel to a muffle furnace at 220°C for combustion, grind the product and heat to 800°C for pre-calcination for 1-2h.
[0032] Preparation method of the above alumina ceramic material:
[0033] Titanium sol-coated alumina powder, nano-silicon dioxide, graphene oxide, yttrium aluminum garnet preformed powder, lanthanum oxide, neodymium oxide, aluminum trifluoride, vanadium oxide, and lithium carbonate are mixed and ball-milled for 10 hours and then dried. 8 wt% PVA aqueous solution is added for granulation. The obtained granules are added into a mold and cold isostatically pressed at 120 MPa for 100 s to obtain a green body. The green body is heated to 800°C at a rate of 20°C / min in an ammonia atmosphere, and after sintering for 4 hours, the ammonia is replaced by air and the temperature is raised to 1650°C at a rate of 2°C / min and sintered for 3 hours.
[0034] Embodiment 2:
[0035] An alumina ceramic material for a thermal quantity sensor comprises the following raw materials in parts by weight:
[0036] 80 parts of titanium sol-coated alumina powder, 30 parts of nano-silicon dioxide, 0.1-0.5 parts of graphene oxide, 20 parts of yttrium aluminum garnet prefabricated powder, 2 parts of lanthanum oxide, 1 part of neodymium oxide, 0.4 parts of aluminum trifluoride, 0.4 parts of vanadium oxide, and 0.2 parts of lithium carbonate.
[0037] The preparation method of titanium sol-coated alumina powder and yttrium aluminum garnet prefabricated powder is the same as that in Example 1.
[0038] Preparation method of the above alumina ceramic material:
[0039] Titanium sol-coated alumina powder, nano-silicon dioxide, graphene oxide, yttrium aluminum garnet pre-powder, lanthanum oxide, neodymium oxide, aluminum trifluoride, vanadium oxide, and lithium carbonate are mixed and ball-milled and granulated, and then cold isostatically pressed to obtain a green body. The green body is heated to 900°C at a rate of 30°C / min in an ammonia atmosphere, and sintered for 5 hours. The ammonia is replaced by air, and the temperature is then raised to 1700°C at a rate of 5°C / min and sintered for 4 hours.
[0040] Embodiment 3:
[0041] An alumina ceramic material for a thermal quantity sensor comprises the following raw materials in parts by weight:
[0042] 60 parts of titanium sol-coated alumina powder, 20 parts of nano-silicon dioxide, 0.1-0.5 parts of graphene oxide, 10 parts of yttrium aluminum garnet prefabricated powder, 2 parts of lanthanum oxide, 1 part of neodymium oxide, 0.4 parts of aluminum trifluoride, 0.4 parts of vanadium oxide, and 0.2 parts of lithium carbonate.
[0043] The preparation method of titanium sol-coated alumina powder and yttrium aluminum garnet prefabricated powder is the same as that in Example 1.
[0044] Preparation method of the above alumina ceramic material:
[0045] Titanium sol-coated alumina powder, nano-silicon dioxide, graphene oxide, yttrium aluminum garnet pre-powder, lanthanum oxide, neodymium oxide, aluminum trifluoride, vanadium oxide, and lithium carbonate are mixed and ball-milled and granulated, and then cold isostatically pressed to obtain a green body. The green body is heated to 800°C at a rate of 10°C / min in an ammonia atmosphere, and sintered for 3 hours. The ammonia is replaced by air, and then the temperature is raised to 1600°C at a rate of 1°C / min and sintered for 2 hours.
[0046] Embodiment 4:
[0047] An alumina ceramic material for a thermal quantity sensor comprises the following raw materials in parts by weight:
[0048] 80 parts of titanium sol-coated alumina powder, 20 parts of nano-silicon dioxide, 0.1-0.5 parts of graphene oxide, 20 parts of yttrium aluminum garnet prefabricated powder, 2 parts of lanthanum oxide, 1 part of neodymium oxide, 0.4 parts of aluminum trifluoride, 0.4 parts of vanadium oxide, and 0.2 parts of lithium carbonate.
[0049] The preparation method of titanium sol-coated alumina powder and yttrium aluminum garnet prefabricated powder is the same as that in Example 1.
[0050] Preparation method of the above alumina ceramic material:
[0051] Titanium sol-coated alumina powder, nano-silicon dioxide, graphene oxide, yttrium aluminum garnet pre-powder, lanthanum oxide, neodymium oxide, aluminum trifluoride, vanadium oxide, and lithium carbonate are mixed and ball-milled and granulated, and then cold isostatically pressed to obtain a green body. The green body is heated to 900°C at a rate of 10°C / min in an ammonia atmosphere, and sintered for 3 hours. The ammonia is replaced by air, and the temperature is then raised to 1700°C at a rate of 5°C / min and sintered for 4 hours.
[0052] Embodiment 5:
[0053] An alumina ceramic material for a thermal quantity sensor comprises the following raw materials in parts by weight:
[0054] 60 parts of titanium sol-coated alumina powder, 30 parts of nano-silicon dioxide, 0.1-0.5 parts of graphene oxide, 10 parts of yttrium aluminum garnet prefabricated powder, 2 parts of lanthanum oxide, 1 part of neodymium oxide, 0.4 parts of aluminum trifluoride, 0.4 parts of vanadium oxide, and 0.2 parts of lithium carbonate.
[0055] The preparation method of titanium sol-coated alumina powder and yttrium aluminum garnet prefabricated powder is the same as that in Example 1.
[0056] Preparation method of the above alumina ceramic material:
[0057] Titanium sol-coated alumina powder, nano-silicon dioxide, graphene oxide, yttrium aluminum garnet preformed powder, lanthanum oxide, neodymium oxide, aluminum trifluoride, vanadium oxide, and lithium carbonate are mixed and ball-milled and granulated, and then cold isostatically pressed to obtain a green body. The green body is heated to 800°C at a rate of 30°C / min in an ammonia atmosphere, and sintered for 5 hours. The ammonia is replaced by air, and the temperature is then raised to 1700°C at a rate of 1°C / min and sintered for 2 hours.
[0058] Comparative Example 1:
[0059] The method is basically the same as Example 1, except that alumina powder is directly added without being coated with titanium sol.
[0060] Comparative Example 2:
[0061] The method is basically the same as Example 1, except that no nano silicon dioxide is added.
[0062] Comparative Example 3:
[0063] It is basically the same as Example 1, except that graphene oxide is not added.
[0064] Comparative Example 4:
[0065] The method is basically the same as Example 1, except that the yttrium aluminum garnet preformed powder is not added.
[0066] Performance Test:
[0067] The alumina ceramic materials prepared in Examples 1-5 of the present invention and Comparative Examples 1-4 are used as samples;
[0068] Bending strength test: Tested in accordance with GB / T 6569-2006, loading speed 0.5mm / min, unit: MPa;
[0069] Fracture toughness characterizes the ability of a material to prevent crack propagation and is a quantitative indicator of the toughness of ceramics. After the sample is ground and polished, the fracture toughness of the sample is calculated using the indentation method. Unit: MPa·m 1 / 2 ;
[0070] Thermal shock treatment method: heat the sample to 1100℃ and keep it for 30 minutes, then take it out and air cool it to room temperature, then cool it to -40℃ and keep it for 10 minutes, then take it out and air cool it to room temperature. After repeating this cycle 20 times, test the bending strength and fracture toughness of the sample, and calculate the loss rate of the bending strength and fracture toughness of the sample, unit: %. If cracks visible to the naked eye appear during the test, stop the test and record the number of cycles.
[0071] The performance test results are shown in Table 1:
[0072] Table 1:
[0073]
[0074] It can be seen from Table 1 above that the alumina ceramic material prepared in the present invention has good mechanical properties and good thermal shock resistance. No cracks appear after 20 cycles of hot and cold cycling, and the loss rates of bending strength and fracture toughness are both less than 10%.
[0075] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An alumina ceramic material for a thermal quantity sensor, characterized in that: The following raw materials are included in parts by weight: 60-80 parts of titanium sol-coated alumina powder, 20-30 parts of nano-silicon dioxide, 0.1-0.5 parts of graphene oxide, 10-20 parts of yttrium aluminum garnet prefabricated powder, 2-5 parts of rare earth oxide, and 1-3 parts of sintering aid; The preparation method of the titanium sol-coated alumina powder is as follows: After uniformly mixing butyl titanate, acetylacetone and the first portion of anhydrous ethanol, the temperature is raised to 60-70°C, and then a mixture consisting of water, concentrated hydrochloric acid and the second portion of anhydrous ethanol is added dropwise, and stirring is continued until the reaction system gradually changes from a colorless transparent liquid to a light yellow-green sol, and the aluminum oxide powder is mixed with the sol, ball-milled and dried; The preparation method of the yttrium aluminum garnet prefabricated powder is as follows: Add yttrium nitrate, aluminum nitrate and citric acid to a mixed solvent consisting of water and anhydrous ethanol, stir and heat to 65-75°C, keep warm for 1-3 hours, then heat to 85-95°C, continue stirring to evaporate the solvent to obtain a gel, transfer the gel to a muffle furnace at 200-250°C for combustion, grind the obtained product, heat to 750-850°C and pre-calcine for 1-2 hours; The sintering aid comprises aluminum trifluoride, vanadium oxide and lithium carbonate, and the weight ratio of the aluminum trifluoride, vanadium oxide and lithium carbonate is 4-8:4-8:0.5-2; The preparation method of the above-mentioned alumina ceramic material is as follows: Titanium sol-coated alumina powder, nano-silicon dioxide, graphene oxide, yttrium aluminum garnet prefabricated powder, rare earth oxides and sintering aids are mixed and ball-milled to form granules, and then cold isostatically pressed to obtain a green body. The green body is heated to 800-900°C in an ammonia atmosphere, sintered for 3-5 hours, and then the ammonia is replaced by air and heated to 1600-1700°C in a second stage and sintered for 2-4 hours.
2. The alumina ceramic material according to claim 1, characterized in that: The following raw materials are included in parts by weight: 75 parts of titanium sol-coated alumina powder, 25 parts of nano-silicon dioxide, 0.25 parts of graphene oxide, 18 parts of yttrium aluminum garnet prefabricated powder, 3 parts of rare earth oxide, and 1 part of sintering aid.
3. The alumina ceramic material according to claim 1, characterized in that: Acetic acid was added during ball milling.
4. The alumina ceramic material according to claim 1, characterized in that: The ratio of the sum of the amounts of yttrium nitrate and aluminum nitrate to the amount of citric acid is 1:0.6-1.
5. The alumina ceramic material according to claim 1, characterized in that: The rare earth oxide is any one or more combinations of lanthanum oxide, cerium oxide, samarium oxide, neodymium oxide, and yttrium oxide.
6. The alumina ceramic material according to claim 1, characterized in that: The heating rate of the first stage is 10-30℃ / min, and the heating rate of the second stage is 1-5℃ / min.
7. The alumina ceramic material according to claim 5, characterized in that: The rare earth oxides are lanthanum oxide and neodymium oxide, and the weight ratio of the lanthanum oxide to the neodymium oxide is 1-5:1-5.