Dual-phase composite rare earth iron-cobalt magnetic powder with lamellar structure and preparation method thereof

Dual-phase composite rare earth iron-cobalt magnetic powder was prepared by one-step reduction and diffusion method, forming two-phase Sm(Fe,Co)5 and Sm2(Fe,Co)17 phases, solving the natural resonance frequency receptor of traditional magnetic materials in high-frequency environments The problem of limitation has achieved significant improvements in high-frequency magnetic properties and wave absorption properties, simplified the process and reduced material losses.

CN116786832BActive Publication Date: 2024-11-29NANJING UNIV OF SCI & TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310001994.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-03
Publication Date
2024-11-29
Estimated Expiration
2043-01-03

AI Technical Summary

Technical Problem

In the high-frequency electromagnetic wave-absorbing environment, the natural resonance frequency of traditional magnetic wave materials is limited by the Snoek limit, making it difficult to simultaneously improve the natural resonance frequency and initial magnetic permeability. Moreover, the magnetic attenuation of SmCo magnets at high temperatures is smaller than the extension of Fe/Co/Ni magnetic metals. and high frequency magnetic properties.

Method used

A one-step reduction and diffusion method is used to prepare biphasic composite rare earth iron-cobalt magnetic powder with a sheet structure. By regulating the reactant ratio, two phases of Sm(Fe,Co)5 and Sm2(Fe,Co)17 are formed to achieve natural resonance of the multimagnetic phase. Superposition, breaking through the Snoek limit and improving high-frequency magnetic and wave absorption performance.

Benefits of technology

It has achieved the improvement of high-frequency magnetic properties and excellent electromagnetic absorption properties of the material, breaking through the frequency limit of traditional magnetic materials, obtaining layered geometric effect and multi-magnetic phase resonance frequency regulation, simplifying the preparation process, and avoiding powder flattening Irregularity and material loss of chemical machining.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116786832B_ABST
    Figure CN116786832B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of magnetic materials, and specifically relates to a two-phase composite rare earth iron-cobalt magnetic powder with a lamellar structure and a preparation method thereof. The method comprises the following steps: fully mixing and pressing samarium oxide powder, iron oxide powder, cobalt oxide powder, manganese oxide powder, calcium oxide powder, and metal calcium particles of a certain ratio; placing the green body in a tubular furnace with argon and hydrogen to perform a high-temperature reduction diffusion reaction, and naturally cooling to room temperature; crushing, pickling, washing and drying the reaction product to obtain lamellar Sm(Fe,Co)5 and Sm2(Fe,Co) 17 Complex phase rare earth magnetic powder. The present invention can directly obtain lamellar two-phase composite powder, the powder space geometry is controllable, the two-phase ratio is adjustable, and the complex processes of smelting, heat treatment, crushing and powder making of traditional powder metallurgy rare earth magnetic powder are omitted; the composite magnetic powder has good temperature stability, the lamellar two-phase can broaden the absorption bandwidth, and the electromagnetic absorption performance is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of magnetic materials, and in particular relates to a two-phase composite rare earth iron-cobalt magnetic powder with a lamellar structure and a preparation method thereof. Background Art

[0002] In the increasingly popular 5G high-frequency electromagnetic communication environment, the emergence of emerging technologies such as the Internet of Things, unmanned driving, and telemedicine will bring about a more complex space electromagnetic environment, and long-term accumulated high-energy electromagnetic radiation will also harm human health. In addition, the networked fire control radars used to search and track targets in modern warfare mainly operate in the S, C, X, and Ku bands, which also puts forward stringent requirements on the electromagnetic wave absorption capacity of weapons and equipment in the GHz band.

[0003] Most traditional magnetic absorbers (magnetic metals and ferrites) have a natural resonant frequency limited by the Snoek limit (μ i -1)f r When the material is selected, the natural resonance frequency f r and initial magnetic permeability μ i The Snoek limit cannot be improved at the same time, which is also the main bottleneck restricting the high-frequency application of most magnetic materials. In order to break through the frequency limit of material use, researchers turned their attention to the development of "easy-to-surface" high-frequency magnetic materials. The study found that the Snoek limit is not only related to the material's saturation magnetization M s It is proportional to the out-of-plane hard magnetic field H of the material. θ and the in-plane easy magnetic field H s The magnetic moment in the plane is more likely to rotate, and the magnetic permeability is higher. At the same time, since the out-of-plane anisotropy field is much larger than the in-plane anisotropy field, that is, H θ >>H s , the square root of the ratio of the two is >1, which can achieve a breakthrough in the Snoek limit, (μ i -1)f r It can be increased to dozens or even dozens of times of the original, and the high-frequency magnetic properties of the material can be significantly improved. The easy-surface rare earth (RE) material and transition metal (TM) magnetic alloy can simultaneously meet the requirements of the bi-anisotropic model and high M s The RE-TM alloy has higher resistivity and magnetocrystalline anisotropy than the magnetic metals Fe / Co / Ni. At the same time, it induces in-plane anisotropy through flattened shape anisotropy, ensuring the material's good high-frequency magnetic loss capacity and suppressing the high-frequency skin effect of the metal to a certain extent.

[0004] Sm-Co system rare earth magnetic materials have little magnetic attenuation at high temperatures and are irreplaceable high temperature magnetic materials. At present, the most widely used type of 2:17 Sm-Co magnets at home and abroad is Sm2 (Co, Fe, Cu, Zr) 17 Type alloy, the Curie temperature of this type of magnet is about 820-870℃, the temperature coefficient of remanence is about -0.03% / ℃, the temperature coefficient of coercive force is about -0.21% / ℃, and the operating temperature can be as high as about 650℃. The traditional powder metallurgy process for preparing SmCo magnetic powder requires a series of process steps such as alloy smelting, homogenization treatment, crushing and powder making, grading and screening. During the smelting process, the rare earth Sm is easy to volatilize during smelting, resulting in component segregation and a large amount of material burning waste. At the same time, SmCo alloy is "brittle". Unlike metal materials such as Fe / Co / Ni with certain ductility, it is impossible to achieve extreme flattening of powder particles by means of high-energy ball milling. The shape of the absorbing powder in the mechanical crushing process is irregular and the size is large, which also leads to the randomness of the direction of the easy magnetization orientation of the material. Summary of the invention

[0005] The purpose of the present invention is to provide a two-phase composite rare earth iron-cobalt magnetic powder with a lamellar structure and a preparation method thereof, and to achieve controllable preparation of a plurality of magnetic phase composite products by regulating the ratio of reactants, and the superposition of multi-magnetic phase natural resonance can effectively improve the material's wave absorption performance. More importantly, this scheme can directly obtain lamellar wave-absorbing powder materials without the need for powder flattening mechanical processing, breaking through the Snoek limit constraints of traditional magnetic materials and improving the high-frequency application frequency range of the material. Therefore, the lamellar geometric structure effect and multi-magnetic phase resonance frequency regulation can be achieved in one step, and the resulting composite rare earth magnetic material has excellent electromagnetic absorption performance.

[0006] The technical solution to achieve the purpose of the present invention is: a method for preparing a dual-phase composite rare earth iron-cobalt magnetic powder with a lamellar structure, comprising the following steps:

[0007] Step (1): weigh the raw materials in proportion: weigh Sm2O3 powder, mixed powder of Fe2O3 and Co2O3, MnO2 powder, CaO powder and Ca particles in a mass ratio of 5:(9-15):(1-2):(10-20):(16-25);

[0008] Step (2): high temperature heating reduction: the powders weighed in step (1) are mixed and formed into blanks, and then heated to 850-900°C in a mixed atmosphere of Ar and H2 for 2-3 hours, and then heated to 950-1050°C for 1-4 hours, and then cooled in the furnace;

[0009] Step (3): Powdering: The reaction product obtained in step (2) is crushed and ground, and then washed with deionized water, weak acid solution, and ethanol in sequence, and then vacuum dried to obtain Sm(Fe, Co)5 and Sm2(Fe, Co).17 Dual-phase lamellar rare earth magnetic powder.

[0010] Furthermore, the raw materials Sm2O3 powder, Fe2O3 powder, Co2O3 powder, MnO2 powder, CaO powder and Ca particles in step (1) have particle sizes ranging from 0.5 to 1 μm, 1 to 2 μm, 1 to 2 μm, 0.5 to 1 μm, 1 to 2 μm, and 0.5 to 1.5 mm, respectively.

[0011] Furthermore, the density of the green body obtained in step (2) is 2 to 4 g / cm 3 .

[0012] Furthermore, the flow ratio of Ar to H2 in the Ar and H2 mixed atmosphere is 9.5:0.5.

[0013] Furthermore, the weak acid solution in step (3) is a 0.1-0.5 mol / L ammonium chloride solution, and the cleaning time of the weak acid solution is 5-30 min.

[0014] Furthermore, the vacuum drying in step (3) has a drying temperature of 60 to 80° C. and a drying time of 8 to 12 hours.

[0015] A dual-phase composite rare earth iron-cobalt magnetic powder prepared by the above method, the magnetic powder is composed of Sm(Fe, Co)5 and Sm2(Fe, Co) 17 It is composed of two phases, and the magnetic powder has a lamellar geometric morphology.

[0016] Compared with the prior art, the present invention has the following significant advantages:

[0017] 1. Conventional reduction diffusion method can obtain powder particles. The present invention can realize the preparation of lamellar rare earth magnetic materials by one-step reduction diffusion method through the selection of the above-mentioned specific reaction raw materials, the design of the ratio of morphology control agent and dispersant. The scheme is simple and the geometric morphology of magnetic powder is controllable;

[0018] 2. The obtained product is a composite of two magnetic phases, Sm(Fe,Co)5 / Sm2(Fe,Co), and the ratio of the two magnetic phase components can be adjusted according to the ratio of the reaction raw materials;

[0019] 3. For high-frequency magnetic materials, the lamellar shape can effectively increase the natural resonance frequency and break through the frequency limit of the material. At the same time, the dual magnetic phase can realize the superposition of multiple magnetic natural resonances, which can broaden the absorption bandwidth and improve the material's absorption performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Scanning electron microscope micrographs of the magnetic powders obtained in Examples 1 and 2; (a) is Example 1, and (b) is Example 2.

[0021] Figure 2 Magnetic powder diffraction patterns were obtained in Example 1 and Example 2; (a) is Example 1, and (b) is Example 2.

[0022] Figure 3 The electromagnetic absorption properties of magnetic powders were obtained in Examples 1 and 2; (a) is Example 1, and (b) is Example 2. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below in conjunction with the accompanying drawings.

[0024] A lamellar Sm(Fe,Co)5 and Sm2(Fe,Co) 17 Dual-phase rare earth magnetic material and preparation method thereof:

[0025] The reaction raw materials are Sm2O3 powder, mixed powder of Fe2O3 and Co2O3, MnO2 powder, CaO powder and Ca particles which are fully mixed in a specific mass ratio of 5:(9-15):(1-2):(10-20):(16-25). Among them, Sm2O3 and Fe2O3 / Co2O3 are product components, MnO2 is a structure regulator, CaO is a dispersant and Ca is a reducing agent.

[0026] The mixed powder is pressed into a green material, wherein the green material density is 2 to 4 g / cm 3 The green body is placed in a tubular furnace for high temperature heating reduction in a mixed atmosphere of Ar and H2, wherein the flow ratio of Ar to H2 is 9.5:0.5. The furnace temperature is heated to 850-900°C for 2-3 hours, and then continued to be heated to 950-1050°C for 1-4 hours, and then the furnace is cooled.

[0027] The reaction product is crushed and ground, and the powder product obtained is fully ground and cleaned with deionized water, weak acid solution, and ethanol in turn, and vacuum dried to obtain Sm(Fe, Co)5 / Sm2(Fe, Co) two-phase lamellar rare earth magnetic powder.

[0028] The raw materials used are Sm2O3, Fe2O3, Co2O3, MnO2, CaO, and Ca particles, with particle sizes ranging from 0.5 to 1 μm, 1 to 2 μm, 1 to 2 μm, 0.5 to 1 μm, 1 to 2 μm, and 0.5 to 1.5 mm, respectively.

[0029] The weak acid solution used is 0.1-0.5 mol / L ammonium chloride solution, and the cleaning time is 5-30 minutes.

[0030] The drying temperature used is 60-80°C and the drying time is 8-12 hours.

[0031] Example 1

[0032] (1) Weigh 3.5 g Sm2O3, 3.3 g Fe2O3, 3.3 g Co2O3, 0.5 g MnO2, 8.0 g CaO, and 15.0 g Ca and mix them evenly to obtain a precursor.

[0033] (2) The precursor in step (1) is compressed by a tablet press, the pressure is increased to 12 Pa, and the pressure is maintained for 10 minutes to obtain a green body.

[0034] (3) Place the composite green body into a heat-resistant crucible and perform reduction diffusion reaction in a vacuum tube furnace. First, evacuate the tube furnace, introduce argon and hydrogen, and evacuate again. Vacuum for 15 minutes. Repeat twice, and keep a small air flow. The heating rate is 5°C / min, and heat to 850°C and keep it for 2 hours, then continue to heat to 1000°C and keep it for 2 hours. After sintering, cool to room temperature and take out the sample.

[0035] (4) The mixture obtained in step (3) was crushed, and the crushed product was washed with deionized water, 0.1 mol / L ammonium chloride solution, and ethanol in sequence, and stirred for 15 min each. The washed powder was placed in a vacuum drying oven and dried at a set temperature of 60° C. for 12 h.

[0036] After grinding, the lamellar Sm(Fe,Co)5 / Sm2(Fe,Co) 17 Dual-phase rare earth magnetic powder material. The powder micromorphology was obtained by scanning electron microscope observation ( Figure 1 (a)), from Figure 1 As can be seen from (a), the shape of the magnetic powder obtained by the present invention is a lamellar structure; the phase composition structure of the powder obtained by polycrystalline powder diffractometer detection ( Figure 2 (a)), from Figure 2 As can be seen in (a), the magnetic powder includes Sm(Fe,Co)5 and Sm2(Fe,Co) 17 Two phases; the obtained magnetic powder (75% by mass) is mixed with paraffin and pressed into a ring sample. After measuring with a vector grid analyzer, a series of electromagnetic parameters can be obtained, thereby calculating its absorption capacity of electromagnetic waves ( Figure 3 (a)), from Figure 3 (a) It can be seen that the powder has good microwave absorption performance.

[0037] Example 2

[0038] (1) Weigh 3.0 g Sm2O3, 3.0 g Fe2O3, 4.5 g Co2O3, 0.5 g MnO2, 10.0 g CaO, and 12.0 g Ca and mix them evenly to obtain a precursor.

[0039] (2) The precursor in step (1) is compressed by a tablet press, the pressure is increased to 15 Pa, and the pressure is maintained for 10 minutes to obtain a green body.

[0040] (3) Place the composite green body into a heat-resistant crucible and perform reduction diffusion reaction in a vacuum tube furnace. First, evacuate the tube furnace, introduce argon / H2, and evacuate again. Vacuum for 15 minutes. Repeat twice, and keep a small air flow. The heating rate is 5°C / min, and heat to 850°C and keep it for 2 hours, then continue to heat to 1000°C and keep it for 2 hours. After sintering, cool to room temperature and take out the sample.

[0041] (4) The mixture obtained in step (3) is crushed, and the crushed product is washed with deionized water, 0.5 mol / L ammonium chloride solution, and ethanol in sequence, and stirred thoroughly for 20 minutes each. The washed powder is placed in a vacuum drying oven and dried at a set temperature of 80° C. for 10 hours.

[0042] After grinding, the lamellar Sm(Fe,Co)5 / Sm2(Fe,Co) 17 Dual-phase rare earth magnetic powder material. The powder micromorphology was obtained by scanning electron microscope observation ( Figure 1 (b)), it can be seen from the figure that it shows an obvious lamellar structure; the powder phase composition structure ( Figure 2 (b)) proves that the powder is composed of Sm(Fe,Co)5 / Sm2(Fe,Co) 17 The obtained magnetic powder (75% by mass) is mixed with paraffin and pressed into a ring-shaped sample. A series of electromagnetic parameters can be obtained after measurement by a vector grid analyzer, thereby calculating its absorption capacity of electromagnetic waves ( Figure 3 (b)).

[0043] The lamellar Sm(Fe,Co)5 / Sm2(Fe,Co) 17 A dual-phase rare earth magnetic powder material and a preparation method thereof, the material has lamellar and dual-phase advantages, excellent electromagnetic absorption characteristics, and is an ideal high-frequency rare earth-based magnetic material. The preparation method can simultaneously achieve the geometric structure design of lamellar magnetic powder and the matching optimization of multi-magnetic phase performance in one step.

Claims

1. A method for preparing a dual-phase composite rare earth iron-cobalt magnetic powder having a lamellar structure, characterized in that: The steps include: Step (1): weigh the raw materials in proportion: weigh Sm2O3 powder, mixed powder of Fe2O3 and Co2O3, MnO2 powder, CaO powder and Ca particles in a mass ratio of 5:(9-15):(1-2):(10-20):(16-25); Step (2): high temperature heating reduction: the powders weighed in step (1) are mixed and formed into blanks, and then heated to 850-900°C in a mixed atmosphere of Ar and H2 for 2-3 hours, and then heated to 950-1050°C for 1-4 hours, and then cooled in the furnace; Step (3): Powdering: The reaction product obtained in step (2) is crushed and ground, and then washed with deionized water, weak acid solution, and ethanol in sequence, and then vacuum dried to obtain Sm(Fe, Co)5 and Sm2(Fe, Co). 17 Dual-phase lamellar rare earth magnetic powder.

2. The method according to claim 1, characterized in that: The raw materials Sm2O3 powder, Fe2O3 powder, Co2O3 powder, MnO2 powder, CaO powder and Ca particles in step (1) have particle sizes ranging from 0.5 to 1 μm, 1 to 2 μm, 1 to 2 μm, 0.5 to 1 μm, 1 to 2 μm, and 0.5 to 1.5 mm, respectively.

3. The method according to claim 1, characterized in that: The density of the green body obtained in step (2) is 2 to 4 g / cm 3 .

4. The method according to claim 1, characterized in that: The flow ratio of Ar to H2 in the Ar and H2 mixed atmosphere is 9.5:0.

5.

5. The method according to claim 1, characterized in that The weak acid solution in step (3) is a 0.1-0.5 mol / L ammonium chloride solution, and the cleaning time of the weak acid solution is 5-30 min.

6. The method according to claim 1, characterized in that The vacuum drying in step (3) is carried out at a drying temperature of 60 to 80° C. and for a drying time of 8 to 12 hours.

7. A dual-phase composite rare earth iron-cobalt magnetic powder prepared by the method according to any one of claims 1 to 6, characterized in that: The magnetic powder is composed of Sm(Fe,Co)5 and Sm2(Fe,Co) 17 It is composed of two phases, and the magnetic powder has a lamellar geometric morphology.

Citation Information

Patent Citations

  • Samarium-cobalt sintered magnet material and preparation method thereof

    CN101882494A

  • Method for preparing double-phase composite samarium cobalt-iron powder

    CN102416483A