A preparation method of antibacterial plastic wood material and antibacterial floor

Through the use of functional fillers such as modified chitosan and bentonite, the hydrophobicity and flame retardancy of antibacterial wood plastic materials are improved, and the problem of insufficient antibacterial performance of existing materials in humid environments is solved, and multiple properties of the materials are realized promote.

CN116790059BActive Publication Date: 2024-11-19HUIDONG MEIXIN PLASTIC LUMBER PROD MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310931394.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-27
Publication Date
2024-11-19
Estimated Expiration
2043-07-27

AI Technical Summary

Technical Problem

The existing antibacterial wood plastic materials have shortcomings in hydrophobicity and flame retardancy, and it is difficult to maintain long-term use in humid environments while having good antibacterial properties.

Method used

Functional fillers such as modified chitosan and modified bentonite are used to improve the hydrophobicity and flame retardancy of the material through phosphate-equilibrated polyvinyl alcohol and grafting reaction, and enhance the antibacterial properties through the modification of chitosan to form The flame retardant elements of nitrogen, silicon and phosphorus that act in multimolecularly.

Benefits of technology

The hydrophobicity, antibacteriality and flame retardancy of antibacterial wood plastic materials have been improved, and the durability and combustion performance of the material in humid environments are enhanced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a preparation method of an antibacterial plastic wood material and an antibacterial floor. The antibacterial plastic wood material comprises the following raw materials by weight: 20 to 40 parts by weight of wood powder, 2 to 6 parts by weight of isopropoxy tris (dioctyl pyrophosphate acyloxy) titanate, 30 to 40 parts by weight of high-density polyethylene, 20 to 30 parts by weight of linear low-density polyethylene, 10 to 30 parts by weight of functionalized fillers, and 0.35 to 1.2 parts by weight of plastic antibacterial agent. The present invention also provides a preparation method thereof. Compared with the prior art, the antibacterial plastic wood material prepared by the present invention has the advantages of good hydrophobicity, good antibacterial property, good flame retardancy, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer technology, and in particular to a preparation method of an antibacterial plastic-wood material and an antibacterial floor. Background Art

[0002] Wood-plastic composite materials have the characteristics of both plastic and wood. They are an ecological and environmentally friendly material made of "wood" and "plastic" as the main raw materials, and are prepared by melt compounding and extrusion, injection or molding processes. As a green and environmentally friendly material, wood-plastic composite materials are widely used in indoor and outdoor decoration and renovation projects. Wood-plastic composite materials are combustible materials. Their combustion process is divided into a drying preheating stage and a pyrolysis and combustion stage. As the temperature rises to above 500°C, the organic component residues in the wood-plastic composite materials slowly decompose, and the released combustible gas gradually decreases to zero. The decomposition process is basically completed. At this time, the wood-plastic composite material turns to flameless combustion until it is extinguished. Therefore, by mastering the pyrolysis and combustion process of wood-plastic composite materials, it is possible to reasonably select flame retardants, terminate chain reactions, and achieve flame retardancy of materials. The flame retardant treatment of wood-plastic composite materials can be divided into solid phase and gas phase. The solid phase flame retardant treatment is to use flame retardants to dehydrate the system, phase change and other endothermic reactions, reduce the temperature of the combustion area and the substrate, reduce heat, and form a carbon layer to isolate the transfer of heat and oxygen, prevent the escape of combustible gases, and protect the substrate from further impact of flames and heat, such as aluminum / magnesium, boron, and phosphorus flame retardants; in the gas phase, capture the free radicals generated during the combustion process, hinder the exchange of combustible gases and air to terminate various chain reactions, and the released inert gas can also dilute the air, such as halogen flame retardants. Wood-plastic composite materials contain wood fibers, and the materials are easily attacked by fungi. Fungal corrosion is prone to occur in humid environments. Therefore, it is necessary to develop flame-retardant and antibacterial antibacterial wood-plastic materials.

[0003] The invention patent with application number 201210489429.2 discloses a mildew-proof plastic wood material and a preparation method thereof, wherein the mildew-proof plastic wood material comprises the following raw materials by weight: 50-60 parts of recycled HDPE plastic, 130-140 parts of wood powder, 20-30 parts of light calcium carbonate, 6-8 parts of coupling agent, 1-3 parts of zinc stearate, 1-3 parts of EBS, 1-3 parts of paraffin wax, 0.4-0.6 parts of ultraviolet light absorber UV-531, 0.4-0.6 parts of antioxidant 1010, 3-4 parts of iron red 110B, 0.7-0.9 parts of iron brown 66, and 0.6-0.8 parts of carbon black C3113. The mildew-proof plastic wood material has the advantage of not getting moldy when used for a long time in a wet environment, but has poor hydrophobicity.

[0004] The invention patent with application number 202010852487.1 discloses an antibacterial, waterproof, color-change resistant wood-like plastic-wood material and its preparation method. The antibacterial, waterproof, color-change resistant wood-like plastic-wood material includes the following raw materials by weight: 40-60 parts of base material, 40-60 parts of wood powder, 0.4-1.2 parts of coupling agent, 0.1-0.3 parts of antioxidant, 0.1-0.3 parts of light stabilizer, 2-5 parts of compatibilizer, 2-4 parts of composite dispersant, 2-4 parts of antibacterial agent, the base material is composed of HDPE and LEPE in a weight ratio of 1-9:1, and the wood-like plastic-wood material has excellent antibacterial, waterproof, color-change resistant and other properties. However, it has the disadvantage of poor flame retardancy. Summary of the invention

[0005] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to obtain an antibacterial plastic-wood material with good hydrophobicity, flame retardancy and antibacterial properties.

[0006] To achieve the above-mentioned purpose, the present invention provides an antibacterial plastic-wood material, characterized in that it comprises the following raw materials in parts by weight: 20 to 40 parts by weight of wood powder, 2 to 6 parts by weight of isopropoxy tris(dioctyl pyrophosphate) titanate, 30 to 40 parts by weight of high-density polyethylene, 20 to 30 parts by weight of linear low-density polyethylene, 10 to 30 parts by weight of functionalized fillers, and 0.35 to 1.2 parts by weight of plastic antibacterial agent.

[0007] The invention also discloses a method for preparing the antibacterial plastic-wood material.

[0008] A method for preparing an antibacterial plastic wood material comprises the following steps:

[0009] The wood powder and isopropoxy tri(dioctyl pyrophosphate) titanate are mixed, and stirred at 78-83° C. and 2000-3000 rpm for 15-25 minutes to obtain a mixture A; high-density polyethylene, linear low-density polyethylene, functional filler, and plastic antibacterial agent are added to the mixture A, and stirred at 300-500 rpm for 10-20 minutes to obtain a mixture B; the mixture B is extruded and granulated to obtain an antibacterial plastic-wood material.

[0010] Preferably, the extrusion granulation process conditions are: the temperature of zone 1 is 135-165°C, the temperature of zone 2 is 145-175°C, the temperature of zone 3 is 160-190°C, the temperature of zone 4 is 155-185°C, and the screw speed is 20-35 rpm.

[0011] The preparation method of the functionalized filler is:

[0012] Step 1, adding 3-10 parts by weight of chitosan to an acetic acid aqueous solution with a concentration of 0.8-1.2vt%, stirring at 300-500 rpm for 10-30 minutes, then adding acetaldehyde, stirring at 300-500 rpm for 10-30 minutes, then stirring at 300-500 rpm for 45-90 minutes at 65-75° C., cooling to 20-30° C., then adjusting the pH to 9.5-10.5 with a sodium borohydride solution, continuing to stir at 300-500 rpm for 45-90 minutes, filtering, collecting solids, washing with anhydrous ethanol and water for 2-4 times, respectively, extracting with anhydrous ethanol for 2-4 times, collecting solids, and vacuum drying at 45-65° C. for 8-12 hours to obtain primary modified chitosan;

[0013] Step 2, adding 4.5 to 15 parts by weight of sodium hydroxide to 30 to 100 parts by weight of water, and then adding 3 to 10 parts by weight of the primary modified chitosan prepared in step 1, stirring at 300 to 500 rpm for 14 to 20 hours, dripping 18 to 60 parts by weight of a mixed solution of isopropanol and chloroacetic acid at a rate of 10 to 20 mL / min during condensation reflux at 45 to 55° C., and stirring at 300 to 500 rpm for 3 to 5 hours, filtering, collecting solids, dispersing the collected solids in 100 to 400 parts by weight of methanol, adjusting the pH to 6.8 to 7.2 with glacial acetic acid, filtering, collecting solids, washing with anhydrous ethanol and water for 2 to 4 times, respectively, and vacuum drying at 45 to 65° C. for 8 to 12 hours to obtain modified chitosan;

[0014] Step 3, adding 15 to 30 parts by weight of modified bentonite to 500 to 1000 parts by weight of water, stirring at 40 to 60 rpm at 65 to 70° C. for 30 to 60 minutes, cooling to 40 to 60° C. to obtain a mixture C; adding 5 to 20 parts by weight of the modified chitosan prepared in step 2 to an acetone aqueous solution having a concentration of 45 to 55 vt%, stirring at 300 to 500 rpm for 20 to 50 minutes, adjusting the pH to 5.7 to 6.2 with 0.01 to 0.1 mol / L hydrochloric acid, and then adding 5 to 15 parts by weight of 1-(3-dimethyl The method comprises the following steps: adding (a) an aminopropyl)-ethylcarbodiimide hydrochloride and 5 to 15 parts by weight of N-hydroxysuccinimide, stirring at 300 to 500 rpm for 10 to 30 minutes to obtain a mixed solution D; dripping the mixed solution D into the mixture C at a rate of 25 to 35 mL / min under stirring at 40 to 60° C. and 300 to 500 rpm, and then continuing to stir at 40 to 60° C. and 300 to 500 rpm for 22 to 26 hours, cooling to 20 to 30° C., filtering, collecting the solid, washing with water for 2 to 4 times, and freeze-drying to obtain a functionalized filler.

[0015] Preferably, the mass and volume ratio of chitosan to acetic acid aqueous solution in step 1 is 3-10:300-1000 g / mL.

[0016] Preferably, the mass and volume ratio of chitosan to acetaldehyde in step 1 is 3-10:30-100 g / mL.

[0017] Preferably, the sodium borohydride solution in step 1 is prepared by adding 2 to 4 parts by weight of sodium hydroxide to 500 to 750 parts by weight of water, then adding 18 to 30 parts by weight of sodium borohydride, and stirring at 300 to 500 rpm until dissolved.

[0018] Preferably, the mixed solution of isopropanol and chloroacetic acid in step 2 is a mixture in which the mass ratio of isopropanol to chloroacetic acid is 16-25:9-12.

[0019] Preferably, the concentration of glacial acetic acid in step 2 is 17.5 mol / L.

[0020] Preferably, the mass and volume ratio of the modified chitosan to the acetone aqueous solution in step 3 is 5-20:800-3000 g / mL.

[0021] Preferably, the preparation method of the modified bentonite is as follows:

[0022] S1, 2 to 10 parts by weight of polyvinyl alcohol and 20 to 100 parts by weight of water are mixed, stirred at 65 to 70° C. at 300 to 500 rpm for 20 to 50 minutes, then 4 to 20 parts by weight of urea are added, stirred at 85 to 96° C. at 300 to 500 rpm for 20 to 40 minutes, then phosphoric acid with a concentration of 80 to 90 wt% is added dropwise at a rate of 10 to 20 mL / min, and stirring is continued at 85 to 96° C. at 300 to 500 rpm for 2.5 to 4 hours, then cooled to 20 to 30° C., anhydrous ethanol is added, allowed to stand for 2 to 4 hours, filtered, solids are collected, and dried at 75 to 85° C. for 8 to 12 hours to obtain phosphorylated polyvinyl alcohol;

[0023] S2. Mix 15 to 30 parts by weight of bentonite, 0.15 to 0.5 parts by weight of N-(2-aminoethyl)-3-aminopropyltriethoxysilane, and 0.3 to 1 parts by weight of phosphated polyvinyl alcohol, stir at 300 to 500 rpm for 20 to 40 minutes, add 45 to 55vt% ethanol aqueous solution, adjust the pH to 6 to 7 with 0.01 to 0.5 mol / L hydrochloric acid and 0.01 to 0.5 mol / L sodium hydroxide aqueous solution, then ball mill at 400 to 600 rpm for 22 to 26 hours, filter, collect the solid, wash with water 2 to 4 times, dry at 70 to 85° C. for 8 to 12 hours, grind, and pass through a 80 to 150 mesh sieve to obtain modified bentonite.

[0024] Preferably, the mass and volume ratio of the polyvinyl alcohol to phosphoric acid in step S1 is 2-10:3.5-16 g / mL.

[0025] Preferably, the mass and volume ratio of the polyvinyl alcohol to anhydrous ethanol in step S1 is 2-10:170-500 g / mL.

[0026] Preferably, the mass and volume ratio of the bentonite to the ethanol aqueous solution in step S2 is 15-30:35-75 g / mL.

[0027] Preferably, the pore size of the above-mentioned filter membranes is 0.22 to 0.87 microns.

[0028] Preferably, the present invention provides an antibacterial floor, which is prepared by compression molding the antibacterial plastic-wood material prepared above.

[0029] Preferably, the compression molding temperature is 165-185°C.

[0030] Preferably, the compression molding specifications are selected according to the specifications of the antibacterial floor.

[0031] The present invention utilizes the groups on modified chitosan to react with the groups on modified bentonite to prepare a functional filler, and the functional filler is added to a plastic wood material to prepare an antibacterial plastic wood material. The prepared antibacterial plastic wood material has the advantages of good hydrophobicity, good antibacterial effect and good flame retardancy. Grafting phosphate groups onto polyvinyl alcohol can improve the hydrophobicity and flame retardancy of polyvinyl alcohol because the phosphate groups are hydrophobic and flame retardant. At the same time, the intermolecular force of polyvinyl alcohol after phosphate esterification is reduced, which can improve the compatibility of polyvinyl alcohol. Bentonite is flame retardant and has hydroxyl groups. N-(2-aminoethyl)-3-aminopropyltriethoxysilane hydrolyzes the ethoxy groups into silanol groups, which react with the hydroxyl groups on bentonite and phospholipid-modified polyvinyl alcohol, so that N-(2-aminoethyl)-3-aminopropyltriethoxysilane and phospholipid-modified polyvinyl alcohol are grafted onto bentonite, which reduces the surface activity and surface energy of bentonite, improves the dispersibility and hydrophobicity of bentonite, and further improves the flame retardancy of bentonite. Chitosan has antibacterial properties. Chitosan is modified with acetaldehyde and sodium borohydride, and the amino groups on chitosan are converted into methylene groups through reaction. and secondary amine to obtain primary modified chitosan, thereby improving the hydrophobicity of chitosan; then, the primary modified chitosan is carboxymethylated to obtain modified chitosan, wherein the modified chitosan has a carboxyl group, and the modified bentonite has an amino group due to the N-(2-aminoethyl)-3-aminopropyltriethoxysilane, so that the modified chitosan and the amino group on the modified bentonite undergo an acylation reaction to obtain a functional filler, thereby improving the hydrophobicity and antibacterial properties of the functional filler, thereby improving the hydrophobicity and antibacterial properties of the antibacterial wood-plastic material, and at the same time, the nitrogen element contained in the modified chitosan is conducive to the generation of non-combustible gas during combustion, and has an auxiliary effect on improving the flame retardancy of the functional filler, and after the carboxyl group in the modified chitosan is grafted with the amino group in the modified bentonite, a multi-flame retardant element between nitrogen, silicon and phosphorus molecules is formed, thereby further improving the flame retardancy of the modified functional filler, thereby improving the flame retardancy of the antibacterial wood-plastic material.

[0032] Due to the adoption of the above technical scheme, compared with the prior art, the present invention has the following advantages: 1) polyvinyl alcohol is phosphated to obtain phosphated polyvinyl alcohol, phosphorus-based flame retardant elements are introduced, and then the phosphated polyvinyl alcohol and N-(2-aminoethyl)-3-aminopropyltriethoxysilane are grafted on bentonite, thereby improving the hydrophobicity of the bentonite, and the bentonite has flame retardancy. After the phosphated polyvinyl alcohol is grafted, the flame retardancy is further improved, thereby improving the flame retardancy of the antibacterial plastic wood material; 2) chitosan is hydrophobically modified to obtain primary modified chitosan, thereby improving The hydrophobicity of the antibacterial wood-plastic material can be improved, the accumulation of water on the surface of the antibacterial wood-plastic material can be reduced, the humid environment can be reduced, and thus the growth of bacteria on the antibacterial wood-plastic material can be reduced. At the same time, chitosan, as a natural antibacterial agent, has an inhibitory effect on the reproduction of various fungi and bacteria, which can further improve the antibacterial property of the antibacterial wood-plastic material; 3) The primary modified chitosan is carboxymethylated, and then reacted with the amino group on the modified bentonite to obtain a functional filler, and the nitrogen element in the modified chitosan is introduced into the modified bentonite to further improve the flame retardancy of the functional filler, thereby improving the flame retardancy of the antibacterial wood-plastic material. DETAILED DESCRIPTION

[0033] Examples and Comparative Examples Part of the raw material sources:

[0034] Wood powder: Hebei Jiukuo New Materials Co., Ltd., pine wood powder, particle size: 100 mesh, product number: 0130.

[0035] High-density polyethylene: Suzhou Xinlilong Plastic Chemical Co., Ltd., item number: YGH041.

[0036] Linear low-density polyethylene: Suzhou Xinlilong Plastic Chemical Co., Ltd., item number: 2650.

[0037] Plastic antibacterial agent: Guangdong Shunde Lanya Chemical Co., Ltd., model: SY-255.

[0038] Chitosan: Zhengzhou Zhongxin Chemical Products Co., Ltd., deacetylation degree: 94.3, viscosity: 87mPa.s.

[0039] The mixed solution of isopropanol and chloroacetic acid was prepared by mixing 39 g of isopropanol and 20 g of chloroacetic acid, and stirring at 300 rpm for 30 minutes.

[0040] The sodium borohydride solution was prepared by adding 2.5 g of sodium hydroxide to 650 g of water, and then adding 23 g of sodium borohydride, and stirring at 300 rpm until dissolved.

[0041] Polyvinyl alcohol: Shanghai Yingjia Industrial Development Co., Ltd., model: polyvinyl alcohol 1788, item number: 1-7.

[0042] Bentonite: Lingshou County Shuokai Mineral Products Co., Ltd., sodium bentonite, particle size: 325 mesh, item number: 40.

[0043] Example 1

[0044] A method for preparing an antibacterial plastic wood material is as follows:

[0045] 30 g of wood powder and 4 g of isopropoxy tri(dioctyl pyrophosphate) titanate were mixed, and stirred at 80°C and 2500 rpm for 20 minutes to obtain a mixture A; 35 g of high-density polyethylene, 25 g of linear low-density polyethylene, 20 g of functional filler, and 0.65 g of plastic antibacterial agent were added to the mixture A, and stirred at 400 rpm for 15 minutes to obtain a mixture B; the mixture B was extruded and granulated, and the extrusion granulation process conditions were: the temperature of zone 1 was 150°C, the temperature of zone 2 was 160°C, the temperature of zone 3 was 175°C, the temperature of zone 4 was 170°C, and the screw speed was 25 rpm to obtain an antibacterial plastic-wood material.

[0046] The preparation method of the functionalized filler is:

[0047] Step 1, add 8g chitosan to 800mL 1vt% acetic acid aqueous solution, stir at 400 rpm for 20 minutes, then add 80mL acetaldehyde, stir at 400 rpm for 20 minutes, then stir at 70°C and 400 rpm for 60 minutes, cool to 25°C, then adjust the pH to 10 with sodium borohydride solution, continue to stir at 400 rpm for 60 minutes, filter with 0.45 micron filter membrane, collect solid, wash with anhydrous ethanol and water 3 times, extract with anhydrous ethanol 3 times, collect solid, and vacuum dry at 60°C for 10 hours to obtain primary modified chitosan;

[0048] Step 2, add 11.5g of sodium hydroxide to 75g of water, then add 7.5g of the primary modified chitosan prepared in step 1, stir at 400 rpm for 18 hours, add 45g of a mixed solution of isopropanol and chloroacetic acid at a rate of 15mL / min during condensation reflux at 50°C, and stir at 400 rpm for 4 hours, filter with a 0.45 micron filter membrane, collect solids, disperse the collected solids in 350g of methanol, adjust the pH to 7 with 17.5mol / L glacial acetic acid, filter with a 0.45 micron filter membrane, collect solids, wash with anhydrous ethanol and water for 3 times, respectively, and vacuum dry at 60°C for 10 hours to obtain modified chitosan;

[0049] Step 3, adding 20g of modified bentonite to 700g of water, stirring at 68°C and 50 rpm for 45 minutes, cooling to 50°C to obtain a mixture C; adding 10g of the modified chitosan prepared in step 2 to 1500mL of an acetone aqueous solution having a concentration of 50vt%, stirring at 400 rpm for 35 minutes, adjusting the pH to 6 with 0.05mol / L hydrochloric acid, then adding 8g of 1-(3-dimethylaminopropyl)-ethylcarbodiimide hydrochloride and 10g of N-hydroxysuccinimide, stirring at 400 rpm for 20 minutes to obtain a mixed solution D; dripping the mixed solution D into the mixture C at a speed of 30mL / min under stirring at 50°C and 400 rpm, and then continuing to stir at 50°C and 400 rpm for 24 hours, cooling to 25°C, filtering with a 0.45 micron filter membrane, collecting the solid, washing it with water 3 times, and freeze-drying it to obtain a functionalized filler.

[0050] The preparation method of the modified bentonite is as follows:

[0051] S1, 5g polyvinyl alcohol and 50g water were mixed, stirred at 68°C and 400 rpm for 35 minutes, 10g urea was added, stirred at 93°C and 400 rpm for 30 minutes, then 8mL of 85wt% phosphoric acid was added dropwise at a speed of 15mL / min, and the mixture was stirred at 93°C and 400 rpm for 3 hours, then cooled to 25°C, 400mL of anhydrous ethanol was added, and the mixture was allowed to stand for 3 hours, filtered with a 0.45 micron filter membrane, the solid was collected, and dried at 80°C for 10 hours to obtain phosphorylated polyvinyl alcohol;

[0052] S2, 20g bentonite, 0.2g N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 0.4g phosphated polyvinyl alcohol prepared in step S1 were mixed, stirred at 400 rpm for 30 minutes, 50mL of 50vt% ethanol aqueous solution was added, the pH was adjusted to 6.5 with 0.05mol / L hydrochloric acid and 0.05mol / L sodium hydroxide aqueous solution, respectively, and then ball milled at 500 rpm for 24 hours, filtered with a 0.45 micron filter membrane, the solid was collected, washed with water 3 times, dried at 80°C for 10 hours, ground, and passed through a 100 mesh sieve to obtain modified bentonite.

[0053] Comparative Example 1

[0054] The preparation method of an antibacterial plastic wood material is basically the same as that of Example 1, the only difference being that the preparation method of the functional filler is different.

[0055] The preparation method of the functionalized filler is:

[0056] Step 1, add 11.5g sodium hydroxide to 75g water, then add 7.5g chitosan, stir at 400 rpm for 18 hours, add 45g of a mixed solution of isopropanol and chloroacetic acid at a rate of 15mL / min during condensation reflux at 50°C, and stir at 400 rpm for 4 hours, filter with a 0.45 micron filter membrane, collect solids, disperse the collected solids in 350g methanol, adjust the pH to 7 with 17.5mol / L glacial acetic acid, filter with a 0.45 micron filter membrane, collect solids, wash with anhydrous ethanol and water for 3 times, respectively, and vacuum dry at 60°C for 10 hours to obtain modified chitosan;

[0057] Step 2, adding 20g of modified bentonite to 700g of water, stirring at 68°C and 50 rpm for 45 minutes, cooling to 50°C to obtain a mixture C; adding 10g of the modified chitosan prepared in step 2 to 1500mL of an acetone aqueous solution with a concentration of 50vt%, stirring at 400 rpm for 35 minutes, adjusting the pH to 6 with 0.05mol / L hydrochloric acid, then adding 8g of 1-(3-dimethylaminopropyl)-ethylcarbodiimide hydrochloride and 10g of N-hydroxysuccinimide, stirring at 400 rpm for 20 minutes to obtain a mixed solution D; dripping the mixed solution D into the mixture C at a speed of 30mL / min under stirring at 50°C and 400 rpm, and then continuing to stir at 50°C and 400 rpm for 24 hours, cooling to 25°C, filtering with a 0.45 micron filter membrane, collecting the solid, washing it with water 3 times, and freeze-drying it to obtain a functionalized filler.

[0058] The preparation method of the modified bentonite is the same as that of Example 1.

[0059] Comparative Example 2

[0060] A method for preparing an antibacterial plastic wood material is as follows:

[0061] 30g of wood powder and 4g of isopropoxy tri(dioctyl pyrophosphate) titanate were mixed, and stirred at 80°C and 2500 rpm for 20 minutes to obtain a mixture A; 35g of high-density polyethylene, 25g of linear low-density polyethylene, 20g of modified bentonite, and 0.65g of plastic antibacterial agent were added to the mixture A, and stirred at 400 rpm for 15 minutes to obtain a mixture B; the mixture B was extruded and granulated, and the extrusion granulation process conditions were: the temperature of zone 1 was 150°C, the temperature of zone 2 was 160°C, the temperature of zone 3 was 175°C, the temperature of zone 4 was 170°C, and the screw speed was 25 rpm to obtain an antibacterial plastic-wood material.

[0062] The preparation method of the modified bentonite is the same as that of Example 1.

[0063] Comparative Example 3

[0064] The preparation method of an antibacterial plastic wood material is basically the same as that of Example 1, the only difference being that the preparation method of the modified bentonite is different.

[0065] The preparation method of the modified bentonite is as follows: 20g bentonite and 0.2g N-(2-aminoethyl)-3-aminopropyltriethoxysilane are stirred at 400 rpm for 30 minutes, and then 50mL of 50vt% ethanol aqueous solution is added, and the pH is adjusted to 6.5 with 0.05mol / L hydrochloric acid and 0.05mol / L sodium hydroxide aqueous solution respectively, and then ball milled at 500 rpm for 24 hours, filtered with a 0.45 micron filter membrane, solids are collected, washed with water 3 times, dried at 80°C for 10 hours, ground, and passed through a 100-mesh sieve to obtain modified bentonite.

[0066] Comparative Example 4

[0067] The preparation method of an antibacterial plastic wood material is basically the same as that of Example 1, the only difference being that the preparation method of the modified bentonite is different.

[0068] The preparation method of the modified bentonite is as follows:

[0069] S1, 5g polyvinyl alcohol and 50g water were mixed, stirred at 68°C and 400 rpm for 35 minutes, 10g urea was added, stirred at 93°C and 400 rpm for 30 minutes, then 8mL of 85wt% phosphoric acid was added dropwise at a speed of 15mL / min, and the mixture was stirred at 93°C and 400 rpm for 3 hours, then cooled to 25°C, 400mL of anhydrous ethanol was added, and the mixture was allowed to stand for 3 hours, filtered with a 0.45 micron filter membrane, the solid was collected, and dried at 80°C for 10 hours to obtain phosphorylated polyvinyl alcohol;

[0070] S2, 20g bentonite and 0.4g phosphated polyvinyl alcohol prepared in step S1 were mixed, stirred at 400 rpm for 30 minutes, 50mL of 50vt% ethanol aqueous solution was added, the pH was adjusted to 6.5 with 0.05mol / L hydrochloric acid and 0.05mol / L sodium hydroxide aqueous solution, respectively, and then ball milled at 500 rpm for 24 hours, filtered with a 0.45 micron filter membrane, the solid was collected, washed with water 3 times, dried at 80°C for 10 hours, ground, and passed through a 100 mesh sieve to obtain modified bentonite.

[0071] Comparative Example 5

[0072] The preparation method of an antibacterial plastic wood material is basically the same as that of Example 1, the only difference being that the preparation method of the functional filler is different.

[0073] The preparation method of the functionalized filler is:

[0074] Step 1, add 8g chitosan to 800mL 1vt% acetic acid aqueous solution, stir at 400 rpm for 20 minutes, then add 80mL acetaldehyde, stir at 400 rpm for 20 minutes, then stir at 70°C and 400 rpm for 60 minutes, cool to 25°C, then adjust the pH to 10 with sodium borohydride solution, continue to stir at 400 rpm for 60 minutes, filter with 0.45 micron filter membrane, collect solid, wash with anhydrous ethanol and water 3 times, extract with anhydrous ethanol 3 times, collect solid, and vacuum dry at 60°C for 10 hours to obtain primary modified chitosan;

[0075] Step 2, add 11.5g of sodium hydroxide to 75g of water, then add 7.5g of the primary modified chitosan prepared in step 1, stir at 400 rpm for 18 hours, add 45g of a mixed solution of isopropanol and chloroacetic acid at a rate of 15mL / min during condensation reflux at 50°C, and stir at 400 rpm for 4 hours, filter with a 0.45 micron filter membrane, collect solids, disperse the collected solids in 350g of methanol, adjust the pH to 7 with 17.5mol / L glacial acetic acid, filter with a 0.45 micron filter membrane, collect solids, wash with anhydrous ethanol and water for 3 times, respectively, and vacuum dry at 60°C for 10 hours to obtain modified chitosan;

[0076] Step 3, adding 20g of bentonite to 700g of water, stirring at 68°C and 50 rpm for 45 minutes, cooling to 50°C to obtain a mixture C; adding 10g of the modified chitosan prepared in step 2 to 1500mL of an acetone aqueous solution with a concentration of 50vt%, stirring at 400 rpm for 35 minutes, adjusting the pH to 6 with 0.05mol / L hydrochloric acid, then adding 8g of 1-(3-dimethylaminopropyl)-ethylcarbodiimide hydrochloride and 10g of N-hydroxysuccinimide, stirring at 400 rpm for 20 minutes to obtain a mixed solution D; dripping the mixed solution D into the mixture C at a speed of 30mL / min under stirring at 50°C and 400 rpm, and then continuing to stir at 50°C and 400 rpm for 24 hours, cooling to 25°C, filtering with a 0.45 micron filter membrane, collecting the solid, washing it with water 3 times, and freeze-drying it to obtain a functionalized filler.

[0077] Test Example 1

[0078] Hydrophobicity test:

[0079] Referring to the master's thesis (Preparation and Performance Study of Antibacterial Hydrophobic Polyester Fiber Film, Author: Lin Xinghuan, Jiangnan University, 2019), the hydrophobicity test of the antibacterial plastic wood material prepared by the present invention is carried out, and the steps are as follows: first, the antibacterial plastic wood material prepared by the present invention is molded at 170°C into a hydrophobic test specimen with a length of 10 cm, a width of 10 cm, and a thickness of 2 cm. Then, 2 μL of water is dropped on the smooth surface of the antibacterial plastic wood board to test the contact angle of the water drop on the surface of the antibacterial plastic wood board. Three parallel tests are made for each specimen, and the results are averaged, as shown in Table 1.

[0080] Test Example 2

[0081] Antimicrobial test:

[0082] The antibacterial plastic wood material prepared by the present invention is molded at 170° C. into a sample with a length of 50 mm, a width of 50 mm, and a thickness of 4 mm as a sample, and the sample is subjected to an antibacterial test with reference to Appendix A "Test Method for Antibacterial Performance" of JC / T2039-2010 "Antibacterial and Mildew-Proof Wood Decorative Panels", wherein the blank control sample is the antibacterial plastic wood material prepared without adding functional fillers, and Staphylococcus aureus is used as the target bacterial species, Staphylococcus aureus (CGMCC: 1.282), and the test results are shown in Table 1.

[0083] Test Example 3

[0084] Limiting oxygen index test:

[0085] According to the national standard of the People's Republic of China GB / T2406.2-2009 "Determination of Combustion Behavior of Plastics by Oxygen Index Method Part 2: Room Temperature Samples", the antibacterial plastic wood material prepared by the present invention is subjected to a limiting oxygen test. The antibacterial plastic wood material prepared by the present invention is molded at 170°C into a sample with a length of 100 mm, a width of 180 mm, and a thickness of 4 mm, and then 16 specimens with a length of 100 mm, a width of 10 mm, and a thickness of 4 mm are cut from the board as samples. During the test, the height of the combustion tube is 500 mm, the inner diameter is 80 mm, and the exhaust flow rate of the limiting hole is 100 mm / s. The top surface ignition test mark and the top surface ignition method are used to ignite the sample. 16 parallels are made for each sample, and the results are averaged, as shown in Table 1.

[0086] Table 1 Test results

[0087] Sample Contact angle / degree Antibacterial rate% Limiting oxygen index % Example 1 32.1 90.47 31.2 Comparative Example 1 29.5 90.12 30.9 Comparative Example 2 29.3 69.15 28.5 Comparative Example 3 28.7 90.12 23.2. Comparative Example 4 28.2 90.08 29.5 Comparative Example 5 26.1 90.09 23.2

[0088] (Note: The smaller the contact angle, the better the hydrophobicity; the larger the limiting oxygen index, the better the flame retardancy)

[0089] By comparing Example 1 with Comparative Examples 1 to 5, it can be found that the hydrophobicity, antibacterial property and flame retardancy of Example 1 are all better than those of Comparative Examples 1 to 5. This may be because the phosphate groups are grafted onto polyvinyl alcohol, which improves the hydrophobicity and flame retardancy of polyvinyl alcohol, thereby improving the hydrophobicity and antibacterial property of the antibacterial plastic wood material; N-(2-aminoethyl)-3-aminopropyltriethoxysilane hydrolyzes the ethoxy groups into silanol groups, which react with the hydroxyl groups on bentonite and phospholipid-modified polyvinyl alcohol, thereby reducing the surface activity and surface energy of bentonite and improving the hydrophobicity and antibacterial property of the antibacterial plastic wood material. The dispersibility and hydrophobicity of bentonite further improve the flame retardancy of bentonite, thereby further improving the flame retardancy and hydrophobicity of the antibacterial wood-plastic material; chitosan has antibacterial properties. After the initial modification of chitosan, the hydrophobicity of chitosan is improved, and then it is carboxymethylated to react with the groups on the modified bentonite, thereby improving the hydrophobicity and antibacterial properties of the antibacterial wood-plastic material. At the same time, the carboxyl groups in the modified chitosan are grafted with the amino groups in the modified bentonite to form multiple flame retardant elements between nitrogen, silicon and phosphorus molecules, further improving the flame retardancy of the antibacterial wood-plastic material.

Claims

1. A method for preparing an antibacterial plastic wood material, characterized in that: The steps include: Mix wood powder and isopropoxy tri(dioctyl pyrophosphate acyloxy) titanate, stir at 78-83° C. and 2000-3000 rpm for 15-25 minutes to obtain a mixture A; then add high-density polyethylene, linear low-density polyethylene, functional filler, and plastic antibacterial agent to the mixture A, stir at 300-500 rpm for 10-20 minutes to obtain a mixture B; extrude and granulate the mixture B to obtain an antibacterial plastic-wood material; The mass ratio of the wood powder, isopropoxy tris(dioctyl pyrophosphate acyloxy) titanate, high-density polyethylene, linear low-density polyethylene, functional filler, and plastic antibacterial agent is 20-40:2-6:30-40:20-30:10-30:0.35-1.2; The preparation method of the functionalized filler is: Step 1, adding chitosan to an acetic acid aqueous solution, stirring, then adding acetaldehyde, stirring, then stirring at 65-75° C., cooling, then adjusting the pH with a sodium borohydride solution, continuing to stir, filtering, collecting solids, washing with anhydrous ethanol and water respectively, extracting with anhydrous ethanol, collecting solids, and vacuum drying to obtain primary modified chitosan; the mass and volume ratio of chitosan to the acetic acid aqueous solution is 3-10:300-1000 g / mL; the mass and volume ratio of chitosan to acetaldehyde is 3-10:30-100 g / mL; the sodium borohydride solution is prepared by: dissolving 2-4 parts by weight of sodium hydroxide in 500-750 parts by weight of water, then adding 18-30 parts by weight of sodium borohydride, and stirring at 300-500 rpm until dissolved; Step 2, adding sodium hydroxide to water, and then adding the primary modified chitosan prepared in step 1, stirring for 14 to 20 hours, adding a mixed solution of isopropanol and chloroacetic acid dropwise during condensation reflux at 45 to 55° C., stirring and reacting for 3 to 5 hours, filtering, collecting solids, dispersing the collected solids in methanol, adjusting the pH with glacial acetic acid, filtering, collecting solids, washing with anhydrous ethanol and water respectively, and vacuum drying to obtain modified chitosan; the mass ratio of sodium hydroxide, water, primary modified chitosan, the mixed solution of isopropanol and chloroacetic acid, and methanol is 4.5 to 15:30 to 100:3 to 10:18 to 60:100 to 400; the mixed solution of isopropanol and chloroacetic acid is a mixture of isopropanol and chloroacetic acid in a mass ratio of 16 to 25:9 to 12; Step 3, adding the modified bentonite to water, stirring at 65-70° C., cooling to 40-60° C., to obtain a mixture C; adding the modified chitosan prepared in step 2 to an acetone aqueous solution, stirring, adjusting the pH with hydrochloric acid, and then adding 1-(3-dimethylaminopropyl)-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, stirring to obtain a mixed solution D; dropping the mixed solution D into the mixture C at 40-60° C. and stirring, and then continuing to stir at 40-6 0°C, stirring for 22 to 26 hours, cooling, filtering, collecting solids, washing with water, and freeze-drying to obtain a functionalized filler; the mass ratio of modified bentonite, water, modified chitosan, 1-(3-dimethylaminopropyl)-ethylcarbodiimide hydrochloride, and N-hydroxysuccinimide is 15 to 30:500 to 1000:5 to 20:5 to 15:5 to 15; the mass and volume ratio of modified chitosan to acetone aqueous solution is 5 to 20:800 to 3000 g / mL; The preparation method of the modified bentonite is as follows: S1, 2-10 parts by weight of polyvinyl alcohol and 20-100 parts by weight of water are mixed, stirred at 65-70°C at 300-500 rpm for 20-50 minutes, then 4-20 parts by weight of urea are added, stirred at 85-96°C at 300-500 rpm for 20-40 minutes, then 80-90wt% phosphoric acid is added dropwise at a rate of 10-20mL / min, and stirring is continued at 85-96°C at 300-500 rpm for 2.5-4 hours, then cooled to 20-30°C, anhydrous ethanol is added, allowed to stand for 2-4 hours, filtered, solids are collected, and dried at 75-85°C for 8-12 hours to obtain phosphorylated polyvinyl alcohol; the mass and volume ratio of polyvinyl alcohol to phosphoric acid is 2-10:3.5-16g / mL; the mass and volume ratio of polyvinyl alcohol to anhydrous ethanol is 2-10:170-500g / mL; S2, 15-30 parts by weight of bentonite, 0.15-0.5 parts by weight of N-(2-aminoethyl)-3-aminopropyltriethoxysilane, and 0.3-1 parts by weight of phosphated polyvinyl alcohol are mixed, stirred at 300-500 rpm for 20-40 minutes, then a 45-55vt% ethanol aqueous solution is added, and the pH is adjusted to 6-7 with 0.01-0.5 mol / L hydrochloric acid and 0.01-0.5 mol / L sodium hydroxide aqueous solution, respectively, and then ball milled at 400-600 rpm for 22-26 hours, filtered, and the solid is collected, washed with water for 2-4 times, dried at 70-85° C. for 8-12 hours, ground, and sieved through 80-150 mesh to obtain modified bentonite; The mass and volume ratio of bentonite to ethanol aqueous solution is 15-30:35-75 g / mL.

2. An antibacterial plastic wood material, characterized in that: The antibacterial plastic-wood material is prepared by the method for preparing the antibacterial plastic-wood material as claimed in claim 1.

3. An antibacterial floor, characterized in that: The antibacterial plastic wood material is prepared by compression molding according to claim 2; the compression molding specifications are selected according to the specifications of the antibacterial floor.