A controlled diffusion process for preparing non-dendritic structure of magnesium-aluminum alloy

By using controlled diffusion solidification method in magnesium aluminum alloy, magnesium aluminum alloy melts of different temperatures and mass are mixed to form uniform non-dendrite structure, solving the problem of insufficient combustion and toughness of magnesium alloys, and achieving low cost and high quality Modification of castings with fluidity and high mechanical properties.

CN116790926BActive Publication Date: 2024-11-05JIANGSU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310055797.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-11-05
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

Combustion accidents often occur in magnesium alloys during resin sand-shaped differential die casting, and traditional semi-solid forming technology cannot effectively form thin-walled complex parts, and the toughness and ductility of magnesium-aluminum alloys are poor.

Method used

By mixing two magnesium-aluminum alloy melts of different temperatures and mass without changing the alloy composition, the controlled diffusion solidification method is used to control the composition, temperature, proportion, mixing rate and flow rate of the melt to form a Uniform non-dendrite structure.

Benefits of technology

It reduces the ignition risk of resin sand casting, improves the fluidity and mechanical properties of magnesium-aluminum alloy, and can form thin-walled complex parts, refines grains, reduces thermal cracking and segregation, and improves the strength and toughness of the castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116790926B_ABST
    Figure CN116790926B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of casting, and specifically to a controlled diffusion process for preparing non-dendritic structures of magnesium-aluminum alloys. The present invention obtains a near-liquid phase magnesium-aluminum alloy casting melt by mixing two alloy melts. Compared with traditional casting, the magnesium-aluminum alloy cast by the controlled diffusion solidification method can form fine non-dendrites and refine grains due to its forced convection, which is beneficial to eliminate thermal cracking and segregation, has better shrinkage compensation, and can even eliminate risers to achieve near-net solidification forming. The present invention can reduce the ignition probability of resin sand casting, and at the same time, compared with traditional semi-solid technology, it has good fluidity and low cost, can form thin-walled complex parts, and has broad prospects in the fields of aerospace and automobiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of casting, and in particular to a controlled diffusion process for preparing non-dendritic structure of magnesium-aluminum alloy. Background Art

[0002] As the requirements for lightweight aviation continue to increase, more and more magnesium alloy castings need to be formed by resin sand mold differential pressure casting to meet quality requirements. However, combustion accidents often occur during the magnesium alloy resin sand mold differential pressure casting process. This is mainly due to the pyrolysis of the sand mold binder to form an oxidizing atmosphere that reacts with the melt, causing the melt to burn.

[0003] The ignition point of magnesium alloy is generally above the solidus line. Semi-solid forming can greatly reduce the risk of ignition. Although traditional semi-solid forming can reduce the pouring temperature through pressure filling, its fluidity is poor and it cannot form thin-walled complex parts. Controlled diffusion solidification is a new type of semi-solid forming technology. Compared with traditional semi-solid, it has good fluidity and can be poured by tilting and gravity at normal pressure. Compared with traditional casting technology, it can refine the grains, obtain fine non-dendritic structure, reduce the tendency of hot cracking and segregation, and improve the mechanical properties of castings.

[0004] Mg-Al-Zn cast magnesium alloys are the most widely used commercial magnesium alloys in industry due to their low cost and good castability. However, with the addition of Al and Zn, the hard and brittle Mg 17 Al 12 The presence of metal compounds of this type will increase the strength, but the toughness and ductility of the alloy will be greatly reduced. At home and abroad, the main method to achieve grain refinement and toughening of magnesium alloys is to change the alloy composition. The present invention obtains a fine and uniform non-dendritic structure by mixing two mother solutions of different temperatures, compositions and masses without changing the composition of the alloy itself. Summary of the invention

[0005] The present invention aims at the combustion and toughening problems of magnesium-aluminum alloy in the resin sand casting process and provides a controlled diffusion method for preparing non-dendritic structure of magnesium-aluminum alloy.

[0006] The object of the present invention is to provide a method for preparing the non-dendritic solidification structure of the above-mentioned magnesium-aluminum alloy.

[0007] To achieve the above-mentioned purpose, the technical solution adopted by the magnesium-aluminum alloy of the present invention comprises the following steps:

[0008] Step 1: Use sandpaper and alcohol to clean the surface oxidation and oil stains of pure magnesium, pure aluminum and magnesium-zinc master alloy for smelting, use 99.95% industrial pure magnesium, 99.95% industrial pure aluminum and magnesium-zinc master alloy (Mg-30Zn) as raw materials, prepare low-temperature low-quality alloy melt and high-temperature high-quality alloy melt, and control the composition and temperature of the two alloy melts, mix the two alloy melts according to a certain proportion, mixing rate and flow rate, and then obtain a uniform non-dendritic solidification structure of the target component alloy. The high-temperature high-quality alloy is industrial pure magnesium, and the low-temperature low-quality alloy is a magnesium-aluminum alloy with high aluminum content smelted by industrial pure magnesium, industrial pure aluminum and magnesium-zinc master alloy (Mg-30Zn). The low-temperature low-quality alloy consists of the following mass percentages: 20~50%Al, 1~5%Zn, and the balance is Mg and unavoidable impurities.

[0009] Step 2: Name the crucibles used for melting the high-temperature high-quality alloy and the low-temperature low-quality alloy as Crucible 1 and Crucible 2 respectively. When the two crucibles are preheated to dark red, add the high-temperature high-quality alloy and the low-temperature low-quality alloy into the crucibles respectively, with the mass ratio of the two alloys being 1.5~5.5.

[0010] Step 3: After heating to 400~500℃, introduce protective gas into the two crucibles, using SF 6 and CO 2 The mixed gas is used as a protective gas; the crucible 1 is continuously heated under the protective atmosphere, the temperature is raised to 700-720°C, a refining agent is added for refining and impurity removal, the temperature is controlled to be lowered to the mixing temperature of the high-temperature and high-quality alloy melt for insulation, and a high-temperature and high-quality alloy melt is obtained, and the mixing temperature of the high-temperature and high-quality alloy is 655-670°C.

[0011] Step 4: Use CO 2 With SF 6 Mixed gas is used as protective gas, pure Mg is heated to 720℃ under protective atmosphere, magnesium-zinc master alloy (Mg-30Zn) and pure Al are added to the pure Mg metal solution, and after the latter added metal is completely melted, it is stirred and kept warm at 680~700℃ for 10min, and the temperature is raised to 700~720℃, and refining agent is added for refining and impurity removal to prepare Mg-Al-Zn metal melt, and the temperature is lowered to the mixing temperature of low-temperature low-quality alloy melt to obtain low-temperature low-quality alloy melt, and the mixing temperature of low-temperature low-quality alloy melt is: 440~520℃.

[0012] Step 5: Pour the high-temperature, high-quality alloy melt into the low-temperature, low-quality alloy melt at a pouring speed of 1.2-1.7 m / s and a mixing rate of 20-200 g / s to obtain a magnesium-aluminum alloy melt of the target composition, and finally pour it into a preheated mold to form a casting.

[0013] The contents of pure magnesium and pure aluminum used in the above steps are in mass percentages. The refining agent is RJ-5 flux, and the mass of RJ-5 flux is 1% to 1.5% of the mass of the alloy in the crucible. 6 With CO 2 The output flow rates are 80 mL / min and 0.8 L / min respectively. Beneficial Effects

[0014] (1) The present invention obtains a near-liquid phase magnesium-aluminum alloy casting melt by mixing two alloy melts, which can reduce the probability of ignition of resin sand casting. At the same time, compared with traditional semi-solid technology, it has good fluidity and low cost, and can form thin-walled complex parts. It has broad prospects in the fields of aerospace and automobiles.

[0015] (2) Compared with traditional casting, the magnesium-aluminum alloy cast by controlled diffusion solidification method can form fine non-dendrites due to its forced convection, which can refine the grain size (such as Figure 2 , 3 ), which is beneficial to eliminate hot cracking and segregation, has better shrinkage compensation, and can even eliminate risers to achieve near-net solidification forming. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The gold phase comparison diagram of Example 1 using the conventional casting method near liquidus casting and the controlled diffusion method is shown in (a) conventional casting (near liquidus casting), (b) Example 1. It is obvious that the present invention can form a rounded and uniform non-dendritic structure.

[0017] Figure 2 The metal phase comparison diagram of Example 2 using the conventional casting method near liquidus casting and the controlled diffusion method is shown in (a) conventional casting (near liquidus casting), (b) Example 2. It is obvious that the present invention can form a rounded and uniform non-dendritic structure.

[0018] Figure 3 It is a schematic diagram of the implementation method of the present invention (① crucible resistance furnace, ② crucible 1, ③ crucible 2, ④ stopper, ⑤ high temperature high quality alloy, ⑥ low temperature low quality alloy, ⑦ target alloy, ⑧ mold). Implementation

[0019] The present invention is a magnesium-aluminum alloy cast by a controlled diffusion solidification method, which is obtained by mixing two alloys of different qualities, compositions and temperatures. The optimal composition and structural uniformity can be achieved by controlling the temperature, proportion, mixing rate and liquid flow rate of the high-temperature high-quality alloy melt and the low-temperature low-quality alloy melt during mixing to obtain a non-dendritic solidification structure. The specific process parameter range is shown in the claims.

[0020] The target magnesium-aluminum alloy obtained by mixing in the present invention is composed of the following components in mass percentage: 8.5-9.5% Al, 0.5-1% Zn, and the balance is Mg and inevitable impurities. The magnesium-aluminum alloy is obtained by mixing alloys with different compositions and mass ratios. The technical solution of the present invention is further described below in combination with the master alloy solutions with different compositions. Example

[0021] The controlled diffusion preparation technology of non-dendritic structure of magnesium-aluminum alloy is specifically:

[0022] In this embodiment, the mixing mass ratio of the high-temperature high-quality alloy melt to the low-temperature low-quality melt is 2.5:1, and the compositions of the two alloy melts are as follows:

[0023] High temperature high quality alloy: 99.95 % Mg, the balance being unavoidable impurities.

[0024] Low temperature, low quality alloy: 31.5~32% Al, 2.5~3% Zn, the balance is Mg and unavoidable impurities.

[0025] The target alloy obtained by implementing this scheme is composed of the following components in mass percentage: 8.5~9.5% Al, 0.5~1% Zn, and the balance is Mg and unavoidable impurities. 99.95% industrial pure magnesium, 99.95% industrial pure aluminum and magnesium-zinc master alloy (Mg-30Zn) are used as raw materials, the high-temperature high-quality alloy is pure Mg, and the low-temperature low-quality alloy is a magnesium-aluminum alloy melt-matched with industrial pure Mg, industrial pure Al and magnesium-zinc master alloy (Mg-30Zn). The high-temperature high-quality alloy melt mixing temperature is 665°C, the low-temperature low-quality alloy melt mixing temperature is 450°C, the high-temperature high-quality alloy and the low-temperature low-quality alloy mixing mass ratio is 2.5:1, the mixing rate is 150 g / s, and the mixed liquid flow velocity is 1.4 m / s. The following is obtained: Figure 1 The uniform non-dendritic solidification structure is shown. Example

[0026] The controlled diffusion preparation technology of non-dendritic structure of magnesium-aluminum alloy is specifically:

[0027] In this embodiment, the mixing mass ratio of the high-temperature high-quality alloy melt to the low-temperature low-quality melt is 4.5:1, and the compositions of the two alloy melts are as follows:

[0028] High temperature high quality alloy: 99.95 % Mg, the balance being unavoidable impurities.

[0029] Low temperature, low quality alloy: 49~49.5% Al, 4.5~5% Zn, the balance is Mg and unavoidable impurities.

[0030] The target alloy obtained by implementing this scheme is composed of the following components in mass percentage: 8.5~9.5% Al, 0.5~1% Zn, and the remainder is Mg and unavoidable impurities. 99.95% industrial pure magnesium, 99.95% industrial pure aluminum and magnesium-zinc master alloy (Mg-30Zn) are used as raw materials, the high-temperature high-quality alloy is pure Mg, and the low-temperature low-quality alloy is a magnesium-aluminum alloy melt-matched with industrial pure Mg, industrial pure Al and magnesium-zinc master alloy (Mg-30Zn). The high-temperature high-quality alloy melt mixing temperature is 660°C, the low-temperature low-quality alloy melt mixing temperature is 465°C, the high-temperature high-quality alloy and the low-temperature low-quality alloy mixing mass ratio is 4.5:1, the mixing rate is 100 g / s, and the mixed liquid flow velocity is 1.7 m / s. The following is obtained: Figure 2 The uniform non-dendritic solidification structure is shown.

[0031] Table 1 shows the detailed parameters of the composition, mass ratio and holding temperature of the master alloy before mixing of Examples 1 and 2.

[0032]

Claims

1. A controlled diffusion process for preparing non-dendritic structure of magnesium-aluminum alloy, characterized in that: The specific steps are as follows: Step 1: clean the surface oxidation and oil stains of pure magnesium, pure aluminum and magnesium-zinc master alloy for smelting, use industrial pure magnesium, industrial pure aluminum and magnesium-zinc master alloy as raw materials, prepare low-temperature low-quality alloy melt and high-temperature high-quality alloy melt, and control the composition and temperature of the two alloy melts, mix the two alloy melts according to a certain proportion, mixing rate and flow rate, and then obtain a uniform non-dendritic solidification structure of the target component alloy; the high-temperature high-quality alloy is industrial pure magnesium, and the low-temperature low-quality alloy is a magnesium-aluminum alloy with high aluminum content smelted by industrial pure magnesium, industrial pure aluminum and magnesium-zinc master alloy, and the magnesium-zinc master alloy is Mg-30Zn; the low-temperature low-quality alloy is composed of the following components in mass percentage: 20~50%Al, 1~5%Zn, and the balance is Mg and unavoidable impurities; Step 2: Name the crucibles used for melting the high-temperature high-quality alloy and the low-temperature low-quality alloy as crucible 1 and crucible 2, respectively. When the two crucibles are preheated to dark red, add the high-temperature high-quality alloy and the low-temperature low-quality alloy into the crucibles, respectively. The mass ratio of the high-temperature high-quality alloy to the low-temperature low-quality alloy is 1.5-5.

5. Step 3: After heating to 400-500°C, a protective gas is introduced into the two crucibles; Crucible 1 is continuously heated under the protective atmosphere, the temperature is raised to 700-720°C, a refining agent is added for refining and impurity removal, the temperature is controlled to be lowered to the mixing temperature of the high-temperature and high-quality alloy melt for insulation, and a high-temperature and high-quality alloy melt is obtained, and the mixing temperature of the high-temperature and high-quality alloy melt is 655-670°C; Step 4: heat pure Mg to 720°C under a protective atmosphere, add magnesium-zinc master alloy and pure Al to the pure Mg metal melt, stir and keep warm at 680-700°C after the latter added metal is completely melted, heat to 700-720°C, add refining agent for refining and impurity removal, prepare Mg-Al-Zn metal melt, cool to the mixing temperature of low-temperature low-quality alloy melt, obtain low-temperature low-quality alloy melt, the mixing temperature of low-temperature low-quality alloy melt is: 440-520°C; Step 5: Cast the high-temperature, high-quality alloy melt into the low-temperature, low-quality alloy melt to obtain a magnesium-aluminum alloy melt of the target composition, and finally pour it into a preheated mold to form a casting. The casting is performed at a pouring speed of 1.2~1.7 m / s and a mixing rate of 20~200 g / s.

2. A controlled diffusion process for preparing non-dendritic structure of magnesium-aluminum alloy according to claim 1, characterized in that: In step 1, the surface oxidation and oil stains of pure magnesium, pure aluminum and magnesium-zinc master alloy for smelting are cleaned with sandpaper and alcohol. The content of industrial pure magnesium is 99.95%, and the content of industrial pure aluminum is 99.95%, both of which are mass percentages.

3. The controlled diffusion process for preparing non-dendritic structure of magnesium-aluminum alloy according to claim 1, characterized in that: In step three, a mixed gas of SF6 and CO2 is used as the protective gas, and the output flow rates of SF6 and CO2 are 80 mL / min and 0.8 L / min respectively. The refining agent is RJ-5 flux, and the mass of RJ-5 flux is 1%~1.5% of the mass of the alloy in the crucible.

4. The controlled diffusion process for preparing non-dendritic structure of magnesium-aluminum alloy according to claim 1, characterized in that: In step 4, a mixed gas of SF6 and CO2 is used as the protective gas, the output flow rates of SF6 and CO2 are 80 mL / min and 0.8 L / min respectively, the holding time is 10 min, and the refining agent is RJ-5 flux, the mass of RJ-5 flux is 1%~1.5% of the mass of the alloy in the crucible.

Citation Information

Cited By

  • Method for improving strength and plasticity of low-alloying Mg-Y-based rare earth magnesium alloy

    CN120026197A