Ultra-low temperature denitration catalyst and preparation method thereof

By using components such as niobium, vanadium, zirconium, tin, nickel ferate and nanotitanium dioxide-graphene support in the catalyst, combining rare earth metal salts and coupling agents, a high-activity and high-efficiency ultra-low-temperature denitrification catalyst was prepared, which solved the problem of The existing catalysts have low activity and insufficient toxicity in low temperature environments, which have achieved efficient nitrogen oxide removal and improved mechanical properties.

CN116870922BActive Publication Date: 2024-11-15SHANGHAI HANYU ENVIRONMENTAL PROTECTION MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310832096.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-07
Publication Date
2024-11-15
Estimated Expiration
2043-07-07

AI Technical Summary

Technical Problem

The existing catalysts have low activity and low efficiency in low temperature or ultra-low temperature flue gas environments, and are unable to resist SO2, SO3, ammonium sulfide poisoning, water poisoning and alkali metal poisoning. They are not able to meet the needs of mechanical strength and wear resistance. Requirements for ultra-low emissions of nitrogen oxides in the atmosphere in the electricity industry.

Method used

Niobium, vanadium, zirconium, tin, and nickel ferrite are used as the main active components, neodymium, europium, and ytterbium are used as the co-active components, tungsten and molybdenum are used as the modified components, nanotitanium dioxide-graphene is used as the carrier, combined with rare earth metal salts With specific coupling agents, high-activity, high-efficiency ultra-low-temperature denitrification catalysts are prepared through thermal reduction and calcination processes to enhance the toxicity and mechanical properties of the catalysts.

Benefits of technology

In the low temperature environment of 100-280℃, the activity and denitrification efficiency of the catalyst are significantly improved, the toxicity against SO2, SO3, ammonium sulfide salts, water and alkali metals are enhanced, the mechanical strength and wear resistance are improved, and the non-existent quality is satisfied. Ultra-low emission requirements for nitrogen oxides in the atmosphere in the electricity industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts, and specifically discloses an ultra-low temperature denitration catalyst and a preparation method thereof. The catalyst is prepared from raw materials including nano nickel ferrite powder, nano titanium dioxide-graphene powder, ammonium metavanadate, ammonium niobium oxalate, stannous chloride, zirconium sulfate, zirconium oxychloride, rare earth metal salt, ammonium metatungstate, ammonium heptamolybdate, chopped glass fibers, silane coupling agent alcohol solution, titanate coupling agent, hydroxypropyl methylcellulose (HPMC), acesulfame potassium, polyethylene oxide and magic acid. The catalyst has good resistance to SO2 (or SO3) adsorption, high resistance to ammonium sulfate poisoning, strong resistance to water poisoning, and resistance to alkali (earth) metal poisoning. The honeycomb catalyst has a thin inner wall, high mechanical strength, large specific surface area, and high porosity, and is particularly suitable for use in a low-temperature flue gas environment of 100 to 280° C., and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to an ultra-low temperature denitration catalyst and a preparation method thereof. Background Art

[0002] The global climate has been facing unprecedented threats. We need to develop and promote energy-saving and efficient atmospheric environment management technologies, promote ecologically balanced development, and clarify the strategic tasks of building an ecological civilization. The general tone is to promote green development and promote harmonious coexistence between man and nature.

[0003] China adheres to the basic national policy of saving resources and protecting the environment, and is determined to win the battle against pollution. There is a high degree of homogeneity between atmospheric pollutant emissions and greenhouse gas emissions, so pollution reduction and carbon reduction complement each other and increase efficiency synergistically. Nitrogen oxides, as the main forming substance of haze, are one of the main atmospheric pollutants, and the harm they cause to human health has been deeply recognized. Therefore, it is particularly important to efficiently remove industrial nitrogen oxides, especially NOx in the non-power industry.

[0004] At present, the methods for reducing nitrogen oxide emissions are divided into two categories: one is the technology of controlling the generation of NOx during combustion, called low NOx combustion technology, which mainly controls the generation of NOx in three ways: thermal type, rapid type and combustion type during combustion; although it is relatively simple to reduce the generation of NOx by controlling the combustion process, the denitrification efficiency is not high; the other is post-combustion control, which controls the emission of nitrogen oxides by treating industrial waste gas, namely flue gas denitrification technology, which is characterized by the removal method adopted according to the characteristics of NOx oxidation, reduction and adsorption, including dry flue gas denitrification and wet flue gas denitrification. Dry flue gas denitrification, namely the reduction method, uses a reducing agent (NH3, CH4, etc.) to reduce NOx to N2 and H2O, including selective catalytic reduction technology (SCR), selective non-catalytic reduction technology (SNCR), etc.; although wet denitrification can achieve a certain efficiency, the system is complex, and it consumes a lot of water and produces water pollution, so it is rarely used.

[0005] Selective catalytic reduction technology (SCR) is currently the most efficient, mature and widely used technology for removing nitrogen oxides. The gas formed after the catalyst reaction is harmless. The power industry has used medium and high temperature SCR denitrification technology on a large scale for combustion boiler flue gas, but the V2O5 / TiO2 catalyst used in this technology can only be used in the window temperature range of 300-420℃. It has low activity and low denitrification efficiency in flue gas conditions below 300℃, and it will cause serious and irreversible ammonium sulfate poisoning, water poisoning, and alkaline (earth) metal poisoning.

[0006] The flue gas window temperature of most industrial kilns in non-electric industries does not meet the conditions for medium- and high-temperature SCR denitrification (i.e. 300-420°C), such as sintering machines, pelletizing machines, coke ovens, hot air furnaces, heating furnaces, lime kilns, pickling furnaces in the steel industry, garbage incinerators, biomass boilers, hazardous waste incinerators, RTO furnaces in the waste incineration industry, catalytic cracking furnaces, chemical waste liquid furnaces in the chemical industry, glass kilns and ceramic kilns in the glass and ceramics industry, cement kilns, lime kilns, calcium carbide slag kilns, drying furnaces in the cement industry, forging furnaces, casting furnaces, heat treatment furnaces in the manufacturing industry, etc., the flue gas temperature is mostly 100-280°C. In order to achieve ultra-low emission requirements for nitrogen oxides, the commonly used method is to heat the flue gas to above 300°C through coal gas, natural gas or diesel, and then use medium- and high-temperature SCR methods for denitrification. This technical route consumes a lot of energy for heating and produces alarming carbon emissions. It is a typical high-energy consumption and high-carbon emission "energy consumption and emission reduction" type, which runs counter to the "energy conservation and emission reduction" and "green and low-carbon" environmental protection strategies advocated by my country and the development direction of sustainable green development. For example, sintering machines and pelletizing machines are one of the most important equipment in the steel industry. They are numerous, with large flue gas volumes and flue gas temperatures of 120 to 160°C. Their nitrogen oxides cause great environmental pollution. China's new environmental protection ultra-low emission standard requires NOx≤50mg / Nm 3 If the flue gas is heated to above 300℃, it will consume a staggering amount of energy. 2 The flue gas from the sintering machine is heated to 300℃ for medium-high temperature denitrification, and the amount of mixed gas consumed is about 7700m 3 / h, with an annual consumption of 59.13 million m 3 , based on the mixed gas price of 0.35 yuan / m 3 Calculation shows that the annual gas cost is about 20.7 million yuan, and the annual increase in carbon emissions is about: 59130000*800 / 7000*2.4567=16600 tons. China's crude steel output is more than 900 million tons, and the area of ​​​​the sintering machine supporting it is about 190,000 square meters. The annual gas cost for 300℃ medium and high temperature denitrification heating is preliminarily estimated to be more than 30 billion yuan, and the annual increase in carbon emissions is about 24.3 million tons.

[0007] In view of the characteristics of flue gas in the non-electric industry, it is necessary to solve the ultra-low emission problem of nitrogen oxides and achieve the goal of energy conservation and carbon reduction. The more ideal and practical method is to develop ultra-low temperature catalysts with high activity, high efficiency and excellent anti-poisoning ability under ultra-low temperature environment.

[0008] Existing catalysts generally have the following problems: low activity in low or ultra-low temperature flue gas environments, low efficiency, poor resistance to SO2 (or SO3) adsorption, low resistance to ammonium sulfate poisoning, weak resistance to water poisoning, inability to resist alkali (earth) metal poisoning, poor molding processability, low mechanical strength, and insufficient wear resistance. Summary of the invention

[0009] The purpose of the present invention is to provide an ultra-low temperature catalyst with high activity and high denitrification efficiency in a low temperature or ultra-low temperature flue gas environment. The catalyst has good resistance to SO2 (or SO3) adsorption, high resistance to ammonium sulfate poisoning, strong resistance to water poisoning, and resistance to alkali (earth) metal poisoning. The honeycomb catalyst has a thin inner wall, high mechanical strength, large specific surface area, and high porosity, and is particularly suitable for use in a low temperature flue gas environment of 100 to 280°C.

[0010] To achieve the above object, the technical solution adopted by the present invention is:

[0011] An ultra-low temperature denitration catalyst, comprising the following raw materials in parts by weight:

[0012]

[0013] Preferably, the catalyst is made of the following raw materials in parts by weight:

[0014]

[0015]

[0016] More preferably, the catalyst is made of the following raw materials in parts by weight:

[0017]

[0018]

[0019] Further preferably, the preparation method of the nano titanium dioxide-graphene is:

[0020] (1) mixing graphene oxide and anatase titanium dioxide nanopowder in a mass ratio of 1-3:30-100 to obtain a titanium dioxide / graphene oxide composite;

[0021] (2) The titanium dioxide / graphene oxide composite is thermally reduced at 350-450° C. for 1 h under an inert atmosphere to obtain a titanium dioxide / graphene composite carrier.

[0022] More preferably, the anatase titanium dioxide nanocrystal has a particle size of 2 to 6 nm and a specific surface area of ​​200 to 270 m 2 / g.

[0023] More preferably, the rare earth metal salt consists of 1.5 to 2.5 parts by weight of neodymium nitrate, 1 to 2 parts by weight of europium nitrate and 1 to 2 parts by weight of ytterbium nitrate.

[0024] Further preferably, the grain size of the nano nickel ferrite is 5-20 nm; the wire diameter of the chopped glass fiber is 10-15 μm, the length is 4-5 mm, and the alkali metal oxide is ≤0.8%; the viscosity-average molecular weights of HPMC and polyethylene oxide are 50,000-100,000 and 5,000,000-7,000,000 respectively.

[0025] Further preferably, the silane coupling agent is one of KH540, KH550 and KH560.

[0026] In addition, the present invention also claims a method for preparing the ultra-low temperature denitration catalyst, comprising the following steps:

[0027] (1) 15 to 25 parts by weight of nano nickel ferrite powder, 70 to 80 parts by weight of nano titanium dioxide-graphene powder, 0.5 to 1 parts by weight of octadecanoic acid, 1 to 2 parts by weight of 2,3-hydroxybutanedioic acid, 25 to 35 parts by weight of deionized water, and 5 to 8 parts by weight of aqueous ammonia are sequentially added into a container and stirred to obtain a first mixture;

[0028] (2) adding 1.5 to 2.5 parts by weight of neodymium nitrate, 1 to 2 parts by weight of europium nitrate, and 1 to 2 parts by weight of ytterbium nitrate into 10 to 20 parts of deionized water and dissolving them completely to form a second solution;

[0029] (3) firstly heat 20 to 30 parts by weight of deionized water to 95 to 100° C., then add 1.5 to 2.5 parts by weight of ammonium metavanadate and 0.4 to 0.8 parts by weight of ethanolamine, mix evenly and completely dissolve, then cool to 80° C., then add 3 to 5 parts by weight of ammonium niobium oxalate, 2 to 4 parts by weight of ammonium metatungstate and 4 to 6 parts by weight of ammonium heptamolybdate, and dissolve to obtain a third solution;

[0030] (4) 1.5 to 3 parts by weight of stannous chloride, 1.5 to 3 parts by weight of zirconium sulfate, 1.3 to 2.6 parts by weight of zirconium oxychloride, and 10 to 15 parts by weight of deionized water are uniformly mixed and dissolved to obtain a fourth solution;

[0031] (5) adding the second solution to the first mixture, stirring for 10 to 20 minutes, then adding the third solution and stirring for 20 to 30 minutes, and finally adding the fourth solution, followed by sequentially adding 5 to 7 parts by weight of chopped glass fibers and 0.5 to 1.5 parts by weight of a 0.5 wt% to 2.0 wt% silane coupling agent alcohol solution, 0.5 to 1 parts by weight of a premix of a titanate coupling agent, 1.5 to 3 parts by weight of HPMC, 3 to 5 parts by weight of acesulfame potassium, and 4 to 6 parts by weight of polyethylene oxide, and then stirring and kneading the mixture evenly, and subjecting the mixture to a heating and moisture removal process and kneading for 50 to 100 minutes to form a paste;

[0032] (6) adding 1 to 3 parts by weight of magic acid to the paste prepared in step (5) and kneading for 20 to 30 minutes;

[0033] (7) The paste prepared in step (6) is extruded into a square honeycomb catalyst using an integrated mold, and then dried using steam heating, and calcined by programmed temperature to obtain the ultra-low temperature denitration catalyst.

[0034] Preferably, the concentration of the aqueous ammonia is ≥20wt%.

[0035] Further preferably, the steam heating for drying in step (7) is performed in stages at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C for 24 hours; wherein, the humidity in the drying room is required to be maintained above 80% before reaching 40°C.

[0036] Further preferably, the programmed temperature calcination has a residence time of not less than 3 h and 8 h in the low temperature zone of 120-180 °C and the medium temperature zone of 300-400 °C, respectively, and a residence time of not less than 10 h in the high temperature zone of 480-580 °C.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) The present invention uses niobium, vanadium, zirconium, tin, and nickel ferrite as main active components, neodymium, europium, and ytterbium as auxiliary active components, tungsten and molybdenum as modifying components, and nano-titanium dioxide-graphene powder as a carrier to prepare an ultra-low temperature denitration catalyst with excellent performance. Among them, nickel ferrite can decompose carbon dioxide in flue gas into oxygen and carbon monoxide. Carbon monoxide is a reducing agent and can play a role similar to NH3. Oxygen is very beneficial for denitration; on the other hand, nickel ferrite has certain lattice defects, which can dissociate part of the lattice oxygen to generate oxygen vacancy compounds, and can recapture oxygen to be regenerated and restored. This cycle can be carried out smoothly at a lower temperature; tin is added in the form of stannous chloride, zirconium is added in the form of zirconium sulfate and zirconium oxychloride, and Cl is added while increasing the active elements. - 、SO4 2-Acid radical ions are very beneficial for increasing the amount of acid and the acidity of active sites, which can improve the adsorption capacity and selectivity of NH3, and can also offset the alkali neutralization effect of alkali metals or alkaline earth metals; while neodymium, europium, and ytterbium rare earths can improve the activity, selectivity, and stability of catalysts in low-temperature or ultra-low-temperature flue gas environments. Neodymium, europium, and ytterbium have 2 to 3 valence states, and their oxides not only have strong oxygen supply capacity, which promotes the efficient catalytic reaction, but also their more significant charge characteristics can repel the adsorption of harmful substances such as SO2 (SO3), alkali metals, and heavy metals, thereby significantly reducing the poisoning effect on the catalyst and prolonging the decay period of the catalyst activity. Titanium dioxide-graphene can provide a suitable active component loading surface area and reduce the agglomeration of nanoparticles, thereby improving the low-temperature activity and stability of the catalyst.

[0039] (2) The strong oxidizing property of the highly acidic magic acid added in the present invention is beneficial to help the active elements lose electrons at low temperatures, which is very helpful for improving the catalytic activity; and the combination of HPMC, acesulfame potassium and polyethylene oxide can significantly improve the flexibility, lubricity, rheology, etc. of the mud material, which is particularly important for the extrusion process of thin-walled honeycomb catalysts with high pore counts and high opening rates. The silane coupling agent, titanate coupling agent and chopped glass fiber are premixed and then added to the mud material, which can play a good composite coupling role and produce a synergistic effect, that is, the coupling agent group can chemically react with the inorganic interface and the organic interface respectively, improve the cross-linking effect between the material components, and the coupling effect of the glass fiber treated with the silane coupling agent and the titanate coupling agent is greatly improved, which promotes the bonding level between HPMC, acesulfame potassium, polyethylene oxide and the carrier material and chopped glass fiber, and improves the bonding strength of the carrier material, which is very beneficial for improving the compressive strength, impact strength, shear strength and wear resistance of the finished catalyst. DETAILED DESCRIPTION

[0040] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0041] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0042] Example 1

[0043] A method for preparing an ultra-low temperature denitration catalyst comprises the following steps:

[0044] (1) 15 parts by weight of nano nickel ferrite powder, 80 parts by weight of nano titanium dioxide-graphene powder, 0.5 parts by weight of octadecanoic acid, 2 parts by weight of 2,3-hydroxybutanedioic acid, 25 parts by weight of deionized water, and 8 parts by weight of ammonia water are sequentially added into a container and stirred to obtain a first mixture;

[0045] (2) adding 1.5 parts by weight of neodymium nitrate, 2 parts by weight of europium nitrate, and 1 part by weight of ytterbium nitrate into 10 parts of deionized water and dissolving them completely to form a second solution;

[0046] (3) firstly heat 30 parts by weight of deionized water to 95° C., then add 2.5 parts by weight of ammonium metavanadate and 0.8 parts by weight of ethanolamine, mix evenly and completely dissolve, then cool to 80° C., then add 3 parts by weight of ammonium niobium oxalate, 4 parts by weight of ammonium metatungstate and 4 parts by weight of ammonium heptamolybdate, and dissolve to obtain a third solution;

[0047] (4) 3 parts by weight of stannous chloride, 1.5 parts by weight of zirconium sulfate, 2.6 parts by weight of zirconium oxychloride and 10 parts by weight of deionized water were mixed and dissolved to obtain a fourth solution;

[0048] (5) adding the second solution to the first mixture and stirring for 20 minutes, then adding the third solution and stirring for 20 minutes, and finally adding the fourth solution, followed by sequentially adding 5 parts by weight of chopped glass fiber and 0.5 parts by weight of 1.0 wt% silane coupling agent KH550 ethanol solution, 0.5 parts by weight of a premix of a titanate coupling agent, 3 parts by weight of HPMC, 5 parts by weight of acesulfame potassium, and 6 parts by weight of polyethylene oxide, and then stirring and kneading the mixture evenly, and then heating and dehumidifying the mixture and kneading for 100 minutes to form a paste;

[0049] (6) adding 1 part by weight of magic acid to the paste prepared in step (5) and kneading for 20 minutes;

[0050] (7) The paste prepared in step (6) is extruded into a square honeycomb catalyst using an integrated die, and then dried using steam heating. The catalyst is kept warm for 24 hours at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C, respectively. The ultra-low temperature denitration catalyst is obtained by programmed temperature calcination after the humidity in the drying room is maintained at above 80% at 40°C. The programmed temperature calcination is performed by staying in the low temperature zone of 120-180°C and the medium temperature zone of 300-400°C for 5 hours and 12 hours, respectively, and staying in the high temperature zone of 480-580°C for 15 hours.

[0051] Example 2

[0052] A method for preparing an ultra-low temperature denitration catalyst comprises the following steps:

[0053] (1) adding 25 parts by weight of nano nickel ferrite powder, 70 parts by weight of nano titanium dioxide-graphene powder, 1 part by weight of octadecanoic acid, 1 part by weight of 2,3-hydroxybutanedioic acid, 35 parts by weight of deionized water, and 5 parts by weight of ammonia water into a container in sequence and stirring to obtain a first mixture;

[0054] (2) adding 2.5 parts by weight of neodymium nitrate, 1 part by weight of europium nitrate, and 2 parts by weight of ytterbium nitrate into 20 parts of deionized water and dissolving them completely to form a second solution;

[0055] (3) firstly heat 20 parts by weight of deionized water to 100° C., then add 1.5 parts by weight of ammonium metavanadate and 0.4 parts by weight of ethanolamine, mix evenly and completely dissolve, then cool to 80° C., then add 5 parts by weight of ammonium niobium oxalate, 2 parts by weight of ammonium metatungstate and 6 parts by weight of ammonium heptamolybdate, and dissolve to obtain a third solution;

[0056] (4) 1.5 parts by weight of stannous chloride, 3 parts by weight of zirconium sulfate, 1.3 parts by weight of zirconium oxychloride, and 15 parts by weight of deionized water were mixed and dissolved to obtain a fourth solution;

[0057] (5) adding the second solution to the first mixture and stirring for 10 minutes, then adding the third solution and stirring for 30 minutes, and finally adding the fourth solution, followed by sequentially adding 7 parts by weight of chopped glass fiber and 1.5 parts by weight of 1.0 wt% silane coupling agent KH550 ethanol solution, 1 part by weight of a premix of a titanate coupling agent, 1.5 parts by weight of HPMC, 3 parts by weight of acesulfame potassium, and 4 parts by weight of polyethylene oxide, and then stirring and kneading the mixture evenly, and then heating and dehumidifying the mixture and kneading for 50 minutes to form a paste;

[0058] (6) adding 3 parts by weight of magic acid to the paste prepared in step (5) and kneading for 30 minutes;

[0059] (7) The paste prepared in step (6) is extruded and formed by an integrated mold, and the catalyst is shaped into a square honeycomb. It is then dried by steam heating and kept warm in stages at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C for 24 hours, respectively. The humidity in the drying room is maintained at above 80% before 40°C, and then the ultra-low temperature denitration catalyst is obtained by programmed temperature calcination. The programmed temperature calcination is to stay in the low temperature zone of 120-180°C and the medium temperature zone of 300-400°C for 4 hours and 15 hours, respectively, and stay in the high temperature zone of 480-580°C for 18 hours.

[0060] Example 3

[0061] A method for preparing an ultra-low temperature denitration catalyst comprises the following steps:

[0062] (1) adding 20 parts by weight of nano nickel ferrite powder, 75 parts by weight of nano titanium dioxide-graphene powder, 0.6 parts by weight of octadecanoic acid, 1.5 parts by weight of 2,3-hydroxybutanedioic acid, 30 parts by weight of deionized water, and 6 parts by weight of ammonia water into a container in sequence and stirring to obtain a first mixture;

[0063] (2) adding 2 parts by weight of neodymium nitrate, 1.5 parts by weight of europium nitrate, and 1.5 parts by weight of ytterbium nitrate into 15 parts of deionized water and dissolving them completely to form a second solution;

[0064] (3) firstly heat 25 parts by weight of deionized water to 95° C., then add 2 parts by weight of ammonium metavanadate and 0.6 parts by weight of ethanolamine, mix evenly and completely dissolve, then cool to 80° C., then add 4 parts by weight of ammonium niobium oxalate, 3 parts by weight of ammonium metatungstate and 5 parts by weight of ammonium heptamolybdate, and dissolve to obtain a third solution;

[0065] (4) 2 parts by weight of stannous chloride, 2 parts by weight of zirconium sulfate, 2 parts by weight of zirconium oxychloride, and 12 parts by weight of deionized water are uniformly mixed and dissolved to obtain a fourth solution;

[0066] (5) adding the second solution to the first mixture and stirring for 15 minutes, then adding the third solution and stirring for 25 minutes, and finally adding the fourth solution, followed by sequentially adding 6 parts by weight of chopped glass fiber and 1 part by weight of 1.0 wt% silane coupling agent KH550 ethanol solution, 0.8 parts by weight of a premix of a titanate coupling agent, 2 parts by weight of HPMC, 4 parts by weight of acesulfame potassium, and 5 parts by weight of polyethylene oxide, and then stirring and kneading the mixture evenly, and then heating and dehumidifying the mixture and kneading for 80 minutes to form a paste;

[0067] (6) adding 2 parts by weight of magic acid to the paste prepared in step (5) and kneading for 25 minutes;

[0068] (7) The paste prepared in step (6) is extruded and formed by an integrated mold, and the catalyst is shaped into a square honeycomb. It is then dried by steam heating and heat-insulated for 24 hours at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C, respectively. The humidity in the drying room is maintained at above 80% before 40°C, and then the ultra-low temperature denitration catalyst is obtained by programmed temperature calcination. The programmed temperature calcination is to stay in the low temperature zone of 120-180°C and the medium temperature zone of 300-400°C for 7 hours and 13 hours, respectively, and stay in the high temperature zone of 480-580°C for 17 hours.

[0069] Example 4

[0070] A method for preparing an ultra-low temperature denitration catalyst comprises the following steps:

[0071] (1) 18 parts by weight of nano nickel ferrite powder, 72 parts by weight of nano titanium dioxide-graphene powder, 0.7 parts by weight of octadecanoic acid, 1.5 parts by weight of 2,3-hydroxybutanedioic acid, 25 parts by weight of deionized water, and 6 parts by weight of ammonia water are sequentially added into a container and stirred to obtain a first mixture;

[0072] (2) adding 1.8 parts by weight of neodymium nitrate, 1.5 parts by weight of europium nitrate, and 1.2 parts by weight of ytterbium nitrate into 16 parts of deionized water and dissolving them completely to form a second solution;

[0073] (3) firstly heat 27 parts by weight of deionized water to 95° C., then add 2 parts by weight of ammonium metavanadate and 0.5 parts by weight of ethanolamine, mix evenly and completely dissolve, then cool to 80° C., then add 3.2 parts by weight of ammonium niobium oxalate, 3 parts by weight of ammonium metatungstate and 4 parts by weight of ammonium heptamolybdate, and dissolve to obtain a third solution;

[0074] (4) 2 parts by weight of stannous chloride, 1.8 parts by weight of zirconium sulfate, 1.6 parts by weight of zirconium oxychloride, and 12 parts by weight of deionized water were mixed and dissolved to obtain a fourth solution;

[0075] (5) adding the second solution to the first mixture and stirring for 20 minutes, then adding the third solution and stirring for 20 minutes, and finally adding the fourth solution, followed by sequentially adding 5.5 parts by weight of chopped glass fiber and 0.9 parts by weight of 1.0 wt% silane coupling agent KH550 ethanol solution, 0.7 parts by weight of a premix of a titanate coupling agent, 2 parts by weight of HPMC, 4.8 parts by weight of acesulfame potassium, and 5 parts by weight of polyethylene oxide, and then stirring and kneading the mixture evenly, and then heating and dehumidifying the mixture and kneading for 70 minutes to form a paste;

[0076] (6) adding 1.8 parts by weight of magic acid to the paste prepared in step (5) and kneading for 30 minutes;

[0077] (7) The paste prepared in step (6) is extruded into a square honeycomb catalyst using an integrated die, and then dried using steam heating. The catalyst is kept warm for 24 hours at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C, respectively. The humidity in the drying room is maintained at above 80% before 40°C, and then the catalyst is calcined by programmed temperature increase to obtain the ultra-low temperature denitration catalyst. The programmed temperature increase calcination is performed by staying in the low temperature zone of 120-180°C and the medium temperature zone of 300-400°C for 6 hours and 11 hours, respectively, and staying in the high temperature zone of 480-580°C for 14 hours.

[0078] Comparative Example 1

[0079] A method for preparing an ultra-low temperature denitration catalyst comprises the following steps:

[0080] (1) 20 parts by weight of nano nickel ferrite powder, 75 parts by weight of nano titanium dioxide carrier, 0.6 parts by weight of octadecanoic acid, 1.7 parts by weight of 2,3-hydroxybutanedioic acid, 30 parts by weight of deionized water, and 7 parts by weight of ammonia water are sequentially added into a container and stirred to obtain a first mixture;

[0081] (2) adding 1.2 parts by weight of neodymium nitrate, 1.5 parts by weight of europium nitrate, and 0.8 parts by weight of ytterbium nitrate into 15 parts of deionized water and dissolving them completely to form a second solution;

[0082] (3) firstly heat 25 parts by weight of deionized water to 95° C., then add 1.2 parts by weight of ammonium metavanadate and 0.6 parts by weight of ethanolamine, mix evenly and completely dissolve, then cool to 80° C., then add 2.8 parts by weight of ammonium niobium oxalate, 3.5 parts by weight of ammonium metatungstate and 5.5 parts by weight of ammonium heptamolybdate, and dissolve to obtain a third solution;

[0083] (4) 2 parts by weight of stannous chloride, 2 parts by weight of zirconium sulfate, 2 parts by weight of zirconium oxychloride, and 12 parts by weight of deionized water are uniformly mixed and dissolved to obtain a fourth solution;

[0084] (5) adding the second solution to the first mixture and stirring for 15 minutes, then adding the third solution and stirring for 25 minutes, and finally adding the fourth solution, followed by sequentially adding 4 parts by weight of chopped glass fiber and 1 part by weight of 1.0 wt% silane coupling agent KH550 ethanol solution, 0.8 parts by weight of a premix of a titanate coupling agent, 2 parts by weight of HPMC, 4 parts by weight of acesulfame potassium, and 3.5 parts by weight of polyethylene oxide, and then stirring and kneading the mixture evenly, and then heating and dehumidifying the mixture and kneading for 80 minutes to form a paste;

[0085] (6) adding 2 parts by weight of magic acid to the paste prepared in step (5) and kneading for 25 minutes;

[0086] (7) The paste prepared in step (6) is extruded into a square honeycomb catalyst using an integrated die, and then dried using steam heating. The catalyst is kept warm for 24 hours at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C, respectively. The humidity in the drying room is maintained at above 80% before 40°C, and then the catalyst is calcined by programmed temperature increase to obtain the ultra-low temperature denitration catalyst. The programmed temperature increase calcination is performed by staying in the low temperature zone of 120-180°C and the medium temperature zone of 300-400°C for 6 hours and 9 hours, respectively, and staying in the high temperature zone of 480-580°C for 15 hours.

[0087] Comparative Example 2

[0088] A method for preparing an ultra-low temperature denitration catalyst comprises the following steps:

[0089] (1) adding 75 parts by weight of nano titanium dioxide-graphene powder, 0.6 parts by weight of octadecanoic acid, 1.5 parts by weight of 2,3-hydroxybutanedioic acid, 30 parts by weight of deionized water, and 6 parts by weight of ammonia water into a container in sequence and stirring to obtain a first mixture;

[0090] (2) adding 2 parts by weight of neodymium nitrate, 0.7 parts by weight of europium nitrate, and 1.5 parts by weight of ytterbium nitrate into 15 parts of deionized water and dissolving them completely to form a second solution;

[0091] (3) firstly heat 25 parts by weight of deionized water to 95° C., then add 2 parts by weight of ammonium metavanadate and 0.7 parts by weight of ethanolamine, mix evenly and completely dissolve, then cool to 80° C., then add 4 parts by weight of ammonium niobium oxalate, 1.5 parts by weight of ammonium metatungstate and 3 parts by weight of ammonium heptamolybdate, and dissolve to obtain a third solution;

[0092] (4) 2 parts by weight of stannous chloride, 1 part by weight of zirconium sulfate, 2 parts by weight of zirconium oxychloride, and 12 parts by weight of deionized water are mixed and dissolved to obtain a fourth solution;

[0093] (5) adding the second solution to the first mixture and stirring for 15 minutes, then adding the third solution and stirring for 25 minutes, and finally adding the fourth solution, followed by sequentially adding 6 parts by weight of chopped glass fiber and 0.4 parts by weight of 1.0 wt% silane coupling agent KH550 ethanol solution, 0.8 parts by weight of a premix of a titanate coupling agent, 1.2 parts by weight of HPMC, 4 parts by weight of acesulfame potassium, and 5 parts by weight of polyethylene oxide, and then stirring and kneading the mixture evenly, and then heating and dehumidifying the mixture and kneading for 80 minutes to form a paste;

[0094] (6) adding 1.5 parts by weight of magic acid to the paste prepared in step (5) and kneading for 25 minutes;

[0095] (7) The paste prepared in step (6) is extruded into a square honeycomb catalyst using an integrated die, and then dried using steam heating. The catalyst is kept warm for 24 hours at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C, respectively. The humidity in the drying room is maintained at above 80% before 40°C, and then the catalyst is calcined by programmed temperature increase to obtain the ultra-low temperature denitration catalyst. The programmed temperature increase calcination is performed by staying in the low temperature zone of 120-180°C and the medium temperature zone of 300-400°C for 5 hours and 12 hours, respectively, and staying in the high temperature zone of 480-580°C for 14 hours.

[0096] Comparative Example 3

[0097] A method for preparing an ultra-low temperature denitration catalyst comprises the following steps:

[0098] (1) adding 20 parts by weight of nano nickel ferrite powder, 75 parts by weight of nano titanium dioxide-graphene powder, 1 part by weight of octadecanoic acid, 2 parts by weight of 2,3-hydroxybutanedioic acid, 33 parts by weight of deionized water, and 6 parts by weight of ammonia water into a container in sequence and stirring to obtain a first mixture;

[0099] (2) adding 1.3 parts by weight of neodymium nitrate, 1.5 parts by weight of europium nitrate, and 1.5 parts by weight of ytterbium nitrate into 18 parts of deionized water and dissolving them completely to form a second solution;

[0100] (3) firstly heat 25 parts by weight of deionized water to 95° C., then add 1 part by weight of ammonium metavanadate and 0.6 parts by weight of ethanolamine, mix evenly and completely dissolve, then cool to 80° C., then add 4 parts by weight of ammonium niobium oxalate and 3 parts by weight of ammonium metatungstate, and dissolve to obtain a third solution;

[0101] (4) 2 parts by weight of stannous chloride, 2 parts by weight of zirconium sulfate, 1.1 parts by weight of zirconium oxychloride, and 12 parts by weight of deionized water were mixed and dissolved to obtain a fourth solution;

[0102] (5) adding the second solution to the first mixture and stirring for 15 minutes, then adding the third solution and stirring for 25 minutes, and finally adding the fourth solution, followed by sequentially adding 8 parts by weight of chopped glass fiber and 1 part by weight of 1.0 wt% silane coupling agent KH550 ethanol solution, 0.1 parts by weight of a premix of a titanate coupling agent, 2 parts by weight of HPMC, 2.5 parts by weight of acesulfame potassium, and 5 parts by weight of polyethylene oxide, and then stirring and kneading the mixture evenly, and then heating and dehumidifying the mixture and kneading for 80 minutes to form a paste;

[0103] (6) The paste prepared in step (5) is extruded into a square honeycomb shape by using an integrated mold, and then dried by steam heating. The catalyst is kept warm for 24 hours at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C, respectively. The humidity in the drying room is maintained at above 80% before 40°C, and then the catalyst is calcined by programmed temperature increase to obtain the ultra-low temperature denitration catalyst. The programmed temperature increase calcination is to stay in the low temperature zone of 120-180°C and the medium temperature zone of 300-400°C for 8 hours and 11 hours, respectively, and stay in the high temperature zone of 480-580°C for 16 hours.

[0104] Comparative Example 4

[0105] A method for preparing an ultra-low temperature denitration catalyst comprises the following steps:

[0106] (1) 22 parts by weight of nano nickel ferrite powder, 78 parts by weight of nano titanium dioxide-graphene powder, 0.6 parts by weight of octadecanoic acid, 1.5 parts by weight of 2,3-hydroxybutanedioic acid, 30 parts by weight of deionized water, and 8 parts by weight of ammonia water are sequentially added into a container and stirred to obtain a first mixture;

[0107] (2) adding 2 parts by weight of neodymium nitrate, 1.5 parts by weight of europium nitrate, and 1.5 parts by weight of ytterbium nitrate into 15 parts of deionized water and dissolving them completely to form a second solution;

[0108] (3) firstly heat 25 parts by weight of deionized water to 95° C., then add 1 part by weight of ammonium metavanadate and 0.6 parts by weight of ethanolamine, mix evenly and completely dissolve, then cool to 80° C., then add 4 parts by weight of ammonium niobium oxalate, 5 parts by weight of ammonium metatungstate and 3.5 parts by weight of ammonium heptamolybdate, and dissolve to obtain a third solution;

[0109] (4) adding the second solution to the first mixture and stirring for 15 minutes, then adding the third solution and stirring for 25 minutes, and then sequentially adding 6 parts by weight of chopped glass fiber and 2 parts by weight of 1.0 wt% silane coupling agent KH550 ethanol solution, 0.8 parts by weight of a premix of a titanate coupling agent, 2 parts by weight of HPMC, 4 parts by weight of acesulfame potassium, and 3 parts by weight of polyethylene oxide, and then stirring and kneading the mixture evenly, and then heating and dehumidifying the mixture and kneading for 40 minutes to form a paste;

[0110] (5) adding 2.5 parts by weight of magic acid to the paste prepared in step (4) and kneading for 25 minutes;

[0111] (6) The paste prepared in step (5) is extruded into a square honeycomb catalyst using an integrated mold, and then dried using steam heating. The catalyst is kept warm for 24 hours at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C, respectively. The humidity in the drying room is maintained at above 80% before 40°C, and then the catalyst is calcined by programmed temperature increase to obtain the ultra-low temperature denitration catalyst. The programmed temperature increase calcination is performed by staying in the low temperature zone of 120-180°C and the medium temperature zone of 300-400°C for 4 hours and 10 hours, respectively, and staying in the high temperature zone of 480-580°C for 18 hours.

[0112] The performance tests were performed on the catalysts prepared in Examples 1-4 and Comparative Examples 1-4:

[0113] (1) Denitrification efficiency determination: The simulated flue gas composition is NOx, NH3, O2 and carrier gas N2, with an air velocity of 8000h -1 , NOx concentration is 600ppm, NH3 / NOx molar ratio = 1, O2 concentration: 6%, reaction temperature is controlled at 100-280℃. The flow rate of each gas is controlled by a mass flow meter. Before the gas enters the reactor, it is mixed by a gas mixer and then preheated by a preheater. The NOx concentration at the inlet and outlet is measured by a flue gas analyzer. In order to eliminate the influence of surface adsorption, the system starts collecting and testing after the ventilation operation is stable for 30 minutes.

[0114] (2) Determination of sulfur and water resistance: The simulated flue gas composition is NOx, NH3, SO2, H2O, O2 and carrier gas N2, with an air velocity of 8000h -1 , NOx concentration is 600ppm, NH3 / NOx molar ratio = 1, O2 concentration: 6%, SO2 concentration: 6000ppm, H2O content: 20vol%; reaction temperature is controlled at 150℃. The flow rate of each gas is controlled by a mass flow meter. Before the gas enters the reactor, it is mixed by a gas mixer and then preheated by a preheater. The NOx concentration at the inlet and outlet is measured by a flue gas analyzer. In order to eliminate the influence of surface adsorption, the system starts collecting and testing after the ventilation operation is stable for 30 minutes. The results are shown in the table below.

[0115]

[0116]

[0117] (3) Determination of the strength and wear resistance of the catalyst:

[0118] Three test pieces of each catalyst were cut, with a size of 150mm*150mm*150mm; the axial and radial compressive strength were tested using a pressure testing machine. The wear test method refers to the determination of wear rate in the national standard GB / T38219-2019: two test pieces with a length and width of 65mm and a height of 100mm were cut as test samples and comparison samples; the samples were placed in a constant temperature oven at 105°C and dried for 2 hours, taken out and naturally cooled to room temperature before weighing; the samples were wrapped with kaolin cotton and placed in the sample bin, with a wind speed of 15m / s in the catalyst channel and a wear agent concentration of 50g / m 3 , stop after 2 hours. Take out the sample, put it in an oven at 105℃ to dry for 2 hours, take it out and cool it naturally to room temperature, and weigh it accurately to 0.01g. The wear rate of the blank sample block without adding the reinforcing agent is measured in the same way, and the results are shown in the following table.

[0119]

[0120] The above description is only a preferred specific embodiment of the present invention, and the protection scope of the present invention is not limited thereto. Any simple change or equivalent replacement of the technical solution that can be obviously obtained by any technician familiar with the technical field within the technical scope disclosed in the present invention falls within the protection scope of the present invention.

Claims

1. An ultra-low temperature denitration catalyst, characterized in that: The invention is made of the following raw materials by weight: ; Wherein, the preparation method of the nano titanium dioxide-graphene powder is: (1) mixing graphene oxide and anatase titanium dioxide nanopowder in a mass ratio of 1-3:30-100 to obtain a titanium dioxide / graphene oxide composite; (2) thermally reducing the titanium dioxide / graphene oxide composite at 350-450° C. for 1 h under an inert atmosphere to obtain a titanium dioxide / graphene composite support; Wherein, the preparation of the ultra-low temperature denitration catalyst comprises the following steps: (1) adding nano nickel ferrite powder, nano titanium dioxide-graphene powder, octadecanoic acid, 2,3-hydroxysuccinic acid, deionized water, and ammonia water into a container in sequence and stirring to obtain a first mixture; (2) adding a rare earth metal salt into deionized water and completely dissolving the rare earth metal salt into a second solution; (3) firstly heat the deionized water to 95-100° C., then add ammonium metavanadate and ethanolamine, mix evenly and completely dissolve, then cool to 80° C., then add ammonium niobium oxalate, ammonium metatungstate and ammonium heptamolybdate, and dissolve to obtain a third solution; (4) mixing stannous chloride, zirconium sulfate, zirconium oxychloride and deionized water uniformly and dissolving them to obtain a fourth solution; (5) adding the second solution to the first mixture and stirring for 10 to 20 minutes, then adding the third solution and stirring for 20 to 30 minutes, and finally adding the fourth solution, followed by sequentially adding a premix of chopped glass fiber and 0.5 wt% to 2.0 wt% silane coupling agent alcohol solution, titanate coupling agent, hydroxypropyl methylcellulose, acesulfame potassium, and polyethylene oxide, stirring and kneading the mixture evenly, and then heating and dehumidifying the mixture and kneading for 50 to 100 minutes to form a paste; (6) adding magic acid to the paste prepared in step (5) and kneading for 20 to 30 minutes; (7) The paste prepared in step (6) is extruded into a square honeycomb catalyst using an integrated mold, and then dried using steam heating, and calcined by programmed temperature to obtain the ultra-low temperature denitration catalyst.

2. The ultra-low temperature denitration catalyst according to claim 1, characterized in that: The invention is made of the following raw materials by weight:

3. The ultra-low temperature denitration catalyst according to any one of claims 1 to 2, characterized in that: The invention is made of the following raw materials by weight:

4. The ultra-low temperature denitration catalyst according to claim 1, characterized in that: The anatase titanium dioxide nanocrystal has a particle size of 2 to 6 nm and a specific surface area of ​​200 to 270 m 2 / g.

5. The ultra-low temperature denitration catalyst according to claim 4, characterized in that: The rare earth metal salt consists of neodymium nitrate, europium nitrate and ytterbium nitrate.

6. The ultra-low temperature denitration catalyst according to claim 5, characterized in that: The crystal size of the nano nickel ferrite is 5 to 20 nm; the wire diameter of the chopped glass fiber is 10 to 15 μm, the length is 4 to 5 mm, and the alkali metal oxide is ≤ 0.8%; The viscosity average molecular weights of HPMC and polyethylene oxide are 50,000-100,000 and 5,000,000-7,000,000 respectively.

7. The ultra-low temperature denitration catalyst according to claim 1, characterized in that: The steam heating for drying in step (7) is carried out in stages at 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C and 80°C for 24 hours; wherein, the humidity in the drying room is required to be maintained above 80% before reaching 40°C.

8. The ultra-low temperature denitration catalyst according to claim 1, characterized in that: The programmed temperature calcination in step (7) is performed with a residence time of not less than 3 hours in the low temperature zone of 120-180°C and 8 hours in the medium temperature zone of 300-400°C, and a residence time of not less than 10 hours in the high temperature zone of 480-580°C.