A reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material, preparation method and application thereof
By designing and synthesizing the reduced graphene oxide/hexaazatriphenylene organic composite cathode material, the problem of insufficient cathode material performance in lithium-ion batteries has been solved, achieving high capacity, excellent rate performance and good cycle stability, which has huge potential application value.
Patent Information
- Application Number
- CN202310870961.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-07-17
AI Technical Summary
The capacity and energy density of existing lithium-ion battery cathode materials are close to the limit, and inorganic cathode materials have problems of environmental pollution and resource shortages, and organic small molecule cathode materials have low conductivity and are easy to dissolve, resulting in poor battery rate performance and cycle stability. .
Design and synthesize a reduced graphene oxide/hexaazatriphenylene organic composite cathode material, which is prepared through chemical synthesis methods. It uses the π conjugated structure and high conductivity to increase the density of redox active sites and achieve reversible storage of lithium ions. and excellent electrochemical properties.
It achieves high specific capacity, excellent rate performance and good cycle stability, has huge development potential and application value, simplifies the preparation process and reduces costs.
Smart Images

Figure CN116891569B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion battery materials, and in particular relates to a reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material, a preparation method and application thereof in lithium-ion battery positive electrode materials. Background Art
[0002] Since the 21st century, with the increasing prominence of environmental issues such as the greenhouse effect, the development and storage of green energy has become increasingly important. Lithium-ion batteries have dominated major markets, from portable electronic devices to electric vehicles, and have gradually achieved widespread application. Currently, commercial lithium-ion battery cathode materials are primarily transition metal oxides or phosphates, such as lithium iron phosphate and lithium cobalt oxide. However, their capacity and energy density have reached their limits, making further performance improvements difficult. Furthermore, inorganic cathode materials also face challenges with environmental pollution and resource shortages.
[0003] Compared to inorganic cathode materials, organic cathode materials offer advantages such as low cost, easy processing and synthesis, diverse structures, and the ability to achieve rapid multi-electron redox reactions. Therefore, the synthesis and research of new, high-performance organic cathode materials for lithium-ion batteries is of great significance. n-type organic compounds containing C=N and C=O bonds have been widely used as organic cathode materials for lithium-ion batteries. During the charge and discharge process, the reversible conversion of C=N / CN and C=O / CO, as lithium ions are inserted and extracted, provides battery capacity.
[0004] Organic small molecule cathode materials often suffer from low conductivity and easy solubility in electrolytes, resulting in poor battery rate performance, poor cycling stability, and low energy density and Coulombic efficiency. Polymer backbones have excellent solubility resistance in organic electrolytes, so converting small molecules into polymers is an effective method to improve battery performance. Currently, research on organic polymer cathode materials for lithium-ion batteries is relatively limited. Therefore, the design and synthesis of new organic polymer cathode materials with high specific capacity, high rate performance, high cycling performance, and high energy density holds great scientific and commercial promise. Summary of the Invention
[0005] The present invention aims to provide a reduced graphene oxide / hexaazatriphenylene organic composite cathode material, a preparation method and application thereof in lithium ion battery cathode materials.
[0006] This invention designs and synthesizes a reduced graphene oxide / hexaazatriphenylene organic composite cathode material. Its excellent solvent resistance enables good cycling stability. Its π-conjugated structure and high conductivity facilitate excellent rate performance. The abundant C=N and C=O redox active sites increase the density of these sites, enabling reversible lithium ion storage, high specific capacity, and excellent electrochemical performance. Furthermore, the product is simple to prepare and has significant development potential and application value in the field of lithium-ion battery cathode materials.
[0007] The hexaazatriphenylene polymer of the present invention has the following structural formula:
[0008]
[0009] The preparation method of a hexaazatriphenylene polymer described in the present invention comprises the following chemical synthesis reaction:
[0010]
[0011] The method for preparing the reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material of the present invention comprises the following steps:
[0012] (1) Under a nitrogen atmosphere, cyclohexanone octahydrate and tetraamine monomer are added to a solvent at a molar ratio of 1:0.5-3, with a solid content of 3-5%. After dissolution, 98% concentrated sulfuric acid is added, with a molar ratio of concentrated sulfuric acid to cyclohexanone of 1:1-10; the solution is heated to reflux temperature and stirred for 10-120 hours, cooled to room temperature, and filtered to obtain a black solid;
[0013] (2) The black solid obtained in step (1) was placed in a Soxhlet extractor and extracted with water, acetone, and N-methylpyrrolidone for 20 to 30 hours, respectively. The solid product was then dried under vacuum at 80 to 120° C. for 12 to 36 hours to obtain a hexaazatriphenylene polymer, the structural formula of which is shown below:
[0014]
[0015] R is one or more of the following structural formulas,
[0016]
[0017] (3) The polymer and graphene oxide obtained in step (2) are added to a solvent in a mass ratio of 1:0.5-2, and ultrasonicated for 3-6 times, each time for 20-40 minutes; the dispersed dispersion is placed in a reactor, and the reactor is placed in an oven at 100-200°C for 12-36 hours. After cooling to room temperature, a black solid is obtained by filtering, and the solid product is placed in a vacuum and dried at 80-120°C for 12-36 hours to obtain a reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material.
[0018] (4) The reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material obtained in step (3) is mixed evenly with a conductive agent and a binder in a mortar, and then N-methylpyrrolidone is added as a solvent, and the mixture is stirred for 1 to 2 hours to form a uniform viscous slurry; the slurry is evenly coated on an aluminum foil with a scraper, and vacuum-dried at 40 to 100° C. for 6 to 12 hours to obtain a lithium-ion battery positive electrode sheet, which is cut into a circular sheet with a diameter of 10 mm, and a lithium sheet is used as a counter electrode, and assembled into a CR2032 button battery in an argon-filled glove box.
[0019] Preferably, the tetraamine monomer in step (1) is one or more of 1,2,4,5-tetraaminobenzoquinone, 1,4,6,9-tetraketone-2,3,7,8-tetraaminopyrazine, and 2,3,7,8-tetraaminopyrazine; and the solvent is one or more of water, N-methylpyrrolidone, ethanol, acetic acid, tetrahydrofuran, acetone, methanol, N,N-dimethylformamide, and dimethyl sulfoxide.
[0020] Preferably, the solvent in step (3) is one or more of water, N-methylpyrrolidone, ethanol, acetic acid, tetrahydrofuran, acetone, methanol, N,N-dimethylformamide, and dimethyl sulfoxide.
[0021] Preferably, the binder in step (4) is one or more of polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC), sodium alginate or polyacrylic acid; the conductive agent is acetylene black; the positive electrode material, the conductive agent and the binder are calculated as 100% by mass, wherein the positive electrode material is 40-80%, the conductive agent is 10-50%, and the rest is the binder.
[0022] The reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material described in the present invention has a simple preparation method, the experimental raw materials are cheap and easily available, the polymerization reaction yield is high, and at the same time, it has excellent electrochemical properties such as high capacity, high rate performance, excellent cycle stability and high energy density, which is conducive to large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1: FTIR graph of the hexaazatriphenylene organic polymer prepared in Example 1, the abscissa is the wave number, and the ordinate is the transmittance;
[0024] like Figure 1 As shown, at 1672cm -1 A new peak of C=N stretching vibration appeared at 3300 cm -1 The amino peak intensity at the position was significantly weakened, proving the successful synthesis of the hexaazatriphenylene organic polymer.
[0025] Figure 2 : FTIR graph of the reduced graphene oxide / hexaazatriphenylene organic composite prepared in Example 1, where the abscissa is the wave number and the ordinate is the transmittance;
[0026] like Figure 2 As shown, at 1672cm -1 A new peak of C=N stretching vibration appeared at 3300 cm -1 The amino peak intensity at is significantly weakened, proving the successful synthesis of reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material.
[0027] Figure 3 : SEM image of reduced graphene oxide / hexaazatriphenylene organic composite prepared in Example 1;
[0028] like Figure 3 As shown, in the reduced graphene oxide / hexaazatriphenylene organic composite, reduced graphene oxide and hexaazatriphenylene are well and uniformly dispersed.
[0029] Figure 4 : Cyclic voltammogram of the first five cycles of the reduced graphene oxide / hexaazatriphenylene organic composite prepared in Example 1, where the abscissa is voltage and the ordinate is current;
[0030] like Figure 4 As shown, the battery was subjected to a cyclic voltammetry test, and the CV curves starting from the second cycle were almost identical, indicating that the product of the present invention has good cycle stability.
[0031] Figure 5 : Cyclic stability performance diagram of the reduced graphene oxide / hexaazatriphenylene organic composite battery prepared in Example 1, where the abscissa is the number of cycles and the ordinate is the specific capacity;
[0032] like Figure 5 As shown, the constant current charge and discharge test of the formula battery was carried out. -1 ) at a current density of 207 mA h g -1 , still maintained 174mA hg at 750 laps -1The specific capacity of the product of the present invention shows that the product has excellent cycle stability.
[0033] Figure 6 : Rate performance diagram of the reduced graphene oxide / hexaazatriphenylene organic composite battery prepared in Example 1, where the abscissa is the number of cycles and the ordinate is the specific capacity;
[0034] like Figure 6 As shown, at high current 10C (7882.6mA g -1 ) current density, it still maintains 120mA hg -1 The specific capacity of the product of the present invention shows that the product has very good rate performance.
[0035] The above tests show the excellent electrochemical performance of the reduced graphene oxide / hexaazatriphenylene organic composite as a positive electrode material. DETAILED DESCRIPTION
[0036] The following will clearly and completely describe the technical solutions of the present invention in conjunction with the accompanying drawings. Obviously, the embodiments described are only some of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without any creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] Under a nitrogen atmosphere, 12.48 g of cyclohexanone octahydrate and 18 g of 1,4,6,9-tetraketone-2,3,7,8-tetraaminopyrazine were added to 1000 mL of N-methylpyrrolidone. After dissolution, 15.7 mL of concentrated sulfuric acid (98% by mass) was added. The solution was heated to reflux and stirred for 48 hours. After cooling to room temperature, it was filtered to obtain a black solid. The black solid was placed in a Soxhlet extractor and extracted with water, acetone, and N-methylpyrrolidone for 20 hours respectively. The solid product was then dried under vacuum at 100°C for 24 hours to obtain a hexaazatriphenylene polymer. 14 g of hexaazatriphenylene polymer and 7 g of graphene oxide were added to 3500 mL of water, ultrasonicated 4 times for 30 min each time, and the dispersed dispersion was charged into a reactor. The reactor was placed in an oven at 185°C for 24 h. After cooling to room temperature, the black solid was filtered to obtain the black solid. The solid product was placed in a vacuum and dried at 100°C for 24 h to obtain a reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material.
[0039] The above-mentioned reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material was mixed evenly with acetylene black and PVDF in a mass ratio of 6:3:1 in a mortar, and then N-methylpyrrolidone was added as a solvent, and the mixture was stirred for 1 hour to form a uniform viscous slurry; the slurry was evenly coated on aluminum foil with a spatula and vacuum dried at 80°C for 12 hours to obtain a lithium-ion battery positive electrode sheet, which was cut into a circular sheet with a diameter of 10 mm, and a lithium sheet was used as a counter electrode to assemble a CR2032 button battery in an argon-filled glove box.
[0040] Example 2
[0041] Under a nitrogen atmosphere, 12.48 g of cyclohexanone octahydrate and 18 g of 1,4,6,9-tetraketone-2,3,7,8-tetraaminopyrazine were added to 1000 mL of N-methylpyrrolidone. After dissolution, 15.7 mL of concentrated sulfuric acid (98% by mass) was added. The solution was heated to reflux and stirred for 48 hours. After cooling to room temperature, it was filtered to obtain a black solid. The black solid was placed in a Soxhlet extractor and extracted with water, acetone, and N-methylpyrrolidone for 20 hours respectively. The solid product was then dried under vacuum at 100°C for 24 hours to obtain a hexaazatriphenylene polymer. 7 g of hexaazatriphenylene polymer and 7 g of graphene oxide were added to 3500 mL of water, ultrasonicated 4 times for 30 min each time, and the dispersed dispersion was charged into a reactor. The reactor was placed in an oven at 185°C for 24 h. After cooling to room temperature, the black solid was filtered to obtain the black solid. The solid product was placed in a vacuum and dried at 100°C for 24 h to obtain a reduced graphene oxide / hexaazatriphenylene organic composite.
[0042] The reduced graphene oxide / hexaazatriphenylene organic composite was mixed with acetylene black and PVDF in a mass ratio of 8:1:1 in a mortar. N-methylpyrrolidone was then added as a solvent and stirred for 1 hour to form a uniform, viscous slurry. The slurry was evenly coated onto aluminum foil with a spatula and vacuum-dried at 80°C for 12 hours to obtain a lithium-ion battery positive electrode. The resulting cathode was then cut into 10 mm diameter circular pieces and assembled into CR2032 button cells in an argon-filled glove box using a lithium sheet as the counter electrode. Testing demonstrated similar performance to that of Example 1.
[0043] Example 3
[0044] Under a nitrogen atmosphere, 12.48 g of cyclohexanone octahydrate and 18 g of 1,4,6,9-tetraketone-2,3,7,8-tetraaminopyrazine were added to 1000 mL of N-methylpyrrolidone. After dissolution, 15.7 mL of concentrated sulfuric acid (98% by mass) was added. The solution was heated to reflux and stirred for 48 hours. After cooling to room temperature, it was filtered to obtain a black solid. The black solid was placed in a Soxhlet extractor and extracted with water, acetone, and N-methylpyrrolidone for 20 hours respectively. The solid product was then dried under vacuum at 100°C for 24 hours to obtain a hexaazatriphenylene polymer. 3.5 g of hexaazatriphenylene polymer and 7 g of graphene oxide were added to 3500 mL of water, ultrasonicated 4 times for 30 min each time, and the dispersed dispersion was charged into a reactor. The reactor was placed in an oven at 185°C for 24 h. After cooling to room temperature, the black solid was filtered to obtain the black solid. The solid product was placed in a vacuum and dried at 100°C for 24 h to obtain a reduced graphene oxide / hexaazatriphenylene organic composite.
[0045] The reduced graphene oxide / hexaazatriphenylene organic composite was mixed with acetylene black and PVDF in a mass ratio of 7:2:1 in a mortar. N-methylpyrrolidone was then added as a solvent and stirred for 1 hour to form a uniform, viscous slurry. The slurry was evenly coated onto aluminum foil with a spatula and vacuum-dried at 80°C for 12 hours to obtain a lithium-ion battery positive electrode. The resulting cathode was then cut into 10 mm diameter circular pieces and assembled into CR2032 button cells in an argon-filled glove box using a lithium sheet as the counter electrode. Testing demonstrated similar performance to that of Example 1.
[0046] Example 4
[0047] Under a nitrogen atmosphere, 12.48 g of cyclohexanone octahydrate and 10.8 g of 1,2,4,5-tetraaminobenzoquinone were added to 1000 mL of N-methylpyrrolidone. After dissolution, 15.7 mL of concentrated sulfuric acid (98% by mass) was added. The solution was heated to reflux and stirred for 48 hours. After cooling to room temperature, it was filtered to obtain a black solid. The black solid was placed in a Soxhlet extractor and extracted with water, acetone, and N-methylpyrrolidone for 20 hours respectively. The solid product was then dried under vacuum at 100°C for 24 hours to obtain a hexaazatriphenylene polymer. 14 g of hexaazatriphenylene polymer and 7 g of graphene oxide were added to 3500 mL of water, ultrasonicated 4 times for 30 min each time, and the dispersed dispersion was charged into a reactor. The reactor was placed in an oven at 185°C for 24 h. After cooling to room temperature, the black solid was filtered to obtain the black solid. The solid product was placed in a vacuum and dried at 100°C for 24 h to obtain a reduced graphene oxide / hexaazatriphenylene organic composite.
[0048] The reduced graphene oxide / hexaazatriphenylene organic composite was mixed with acetylene black and PVDF in a mass ratio of 6:3:1 in a mortar. N-methylpyrrolidone was then added as a solvent and stirred for 1 hour to form a uniform, viscous slurry. The slurry was evenly coated onto aluminum foil with a spatula and vacuum-dried at 80°C for 12 hours to obtain a lithium-ion battery positive electrode. The resulting cathode was then cut into 10 mm diameter circular pieces and assembled into CR2032 button cells in an argon-filled glove box using a lithium sheet as the counter electrode. Testing demonstrated similar performance to that of Example 1.
[0049] Example 5
[0050] Under a nitrogen atmosphere, 12.48 g of cyclohexanone octahydrate and 10.8 g of 1,2,4,5-tetraaminobenzoquinone were added to 1000 mL of N-methylpyrrolidone. After dissolution, 15.7 mL of concentrated sulfuric acid (98% by mass) was added. The solution was heated to reflux and stirred for 48 hours. After cooling to room temperature, it was filtered to obtain a black solid. The black solid was placed in a Soxhlet extractor and extracted with water, acetone, and N-methylpyrrolidone for 20 hours respectively. The solid product was then dried under vacuum at 100°C for 24 hours to obtain a hexaazatriphenylene polymer. 14 g of hexaazatriphenylene polymer and 14 g of graphene oxide were added to 3500 mL of water, ultrasonicated 4 times for 30 min each time, and the dispersed dispersion was charged into a reactor. The reactor was placed in an oven at 185°C for 24 h. After cooling to room temperature, the black solid was filtered to obtain the black solid. The solid product was placed in a vacuum and dried at 100°C for 24 h to obtain a reduced graphene oxide / hexaazatriphenylene organic composite.
[0051] The reduced graphene oxide / hexaazatriphenylene organic composite was mixed with acetylene black and PVDF in a mass ratio of 6:3:1 in a mortar. N-methylpyrrolidone was then added as a solvent and stirred for 1 hour to form a uniform, viscous slurry. The slurry was evenly coated onto aluminum foil with a spatula and vacuum-dried at 80°C for 12 hours to obtain a lithium-ion battery positive electrode. The resulting cathode was then cut into 10 mm diameter circular pieces and assembled into CR2032 button cells in an argon-filled glove box using a lithium sheet as the counter electrode. Testing demonstrated similar performance to that of Example 1.
Claims
1. A method for preparing a reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material, the steps of which are as follows: (1) Under a nitrogen atmosphere, cyclohexanone octahydrate and tetraamine monomer are added to a solvent in a molar ratio of 1:0.5-3, with a solid content of 3-5%, and after dissolution, 98% concentrated sulfuric acid is added, with a molar ratio of concentrated sulfuric acid to cyclohexanone of 1:1-10; the solution is heated to reflux temperature and stirred for 10-120 hours, cooled to room temperature, and filtered to obtain a black solid; (2) placing the black solid obtained in step (1) in a Soxhlet extractor, extracting with water, acetone, and N-methylpyrrolidone for 20 to 30 hours respectively, and then drying the solid product in a vacuum at 80 to 120° C. for 12 to 36 hours to obtain a hexaazatriphenylene polymer having the structural formula shown below; (3) adding the polymer and graphene oxide obtained in step (2) to a solvent in a mass ratio of 1:0.5-2, and ultrasonicating for 3-6 times, each time for 20-40 minutes; charging the dispersed liquid into a reactor, placing the reactor in an oven at 100-200° C. for 12-36 hours, cooling to room temperature, and filtering to obtain a black solid, and drying the solid product in a vacuum at 80-120° C. for 12-36 hours to obtain a reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material.
2. The method for preparing a reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material according to claim 1, characterized in that: The solvent in step (1) is one or more of water, N-methylpyrrolidone, ethanol, acetic acid, tetrahydrofuran, acetone, methanol, N,N-dimethylformamide, and dimethyl sulfoxide.
3. The method for preparing a reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material according to claim 1, characterized in that: The solvent in step (3) is one or more of water, N-methylpyrrolidone, ethanol, acetic acid, tetrahydrofuran, acetone, methanol, N,N-dimethylformamide, and dimethyl sulfoxide.
4. A reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material, characterized in that: The method is prepared by any one of claims 1 to 3.
5. Use of the reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material as claimed in claim 4 in positive electrode materials for lithium ion batteries.
6. The use of a reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material as claimed in claim 5 in a positive electrode material for a lithium ion battery, characterized in that: The method comprises the following steps: uniformly mixing the reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material, a conductive agent and a binder in a mortar, and then adding N-methylpyrrolidone as a solvent, and continuing to stir for 1 to 2 hours to mix into a uniform viscous slurry; uniformly coating the slurry on an aluminum foil with a scraper, and vacuum drying at 40 to 100° C. for 6 to 12 hours to obtain a positive electrode sheet of a lithium-ion battery, cutting the sheet into a circular sheet with a diameter of 10 mm, and using a lithium sheet as a counter electrode to assemble into a CR2032 button battery in a glove box filled with argon.
7. The use of a reduced graphene oxide / hexaazatriphenylene organic composite positive electrode material as claimed in claim 6 in a positive electrode material for a lithium ion battery, characterized in that: The binder is one or more of polyvinylidene fluoride, sodium carboxymethyl cellulose, sodium alginate or polyacrylic acid; the conductive agent is acetylene black; the mass sum of the positive electrode material, the conductive agent and the binder is 100%, of which the positive electrode material is 40-80%, the conductive agent is 10-50%, and the rest is the binder.
Citation Information
Patent Citations
Polymer, electrode active material and secondary battery
JP2020066681A
Conductive two-dimensional (2D) covalent organic frameworks (COFS) and method of making an electrode material