Anti-oxidation coating repair material and method for repairing damaged anti-oxidation coating

By using coatings composed of materials such as silicon carbide powder, silicon powder and polycarbosilane, combined with ultra-high temperature ceramic sheet support, the repair problem of large-area damage of ultra-high temperature protective coating of carbon/carbon composite materials is solved, and efficient anti-oxidation is achieved Coating repair extends service life.

CN116903396BActive Publication Date: 2024-11-05SHANGHAI UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310905454.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-21
Publication Date
2024-11-05
Estimated Expiration
2043-07-21

AI Technical Summary

Technical Problem

The prior art is difficult to effectively repair the large-area damage of the ultra-high temperature protective coating of carbon/carbon composite materials, resulting in damage to oxidation under ultra-high temperature conditions and affecting service life.

Method used

An antioxidant coating repair material including a first coating and a second coating is used. The first coating is composed of silicon carbide powder, silicon powder, polycarbonsilane binder and water. The second coating is composed of carbide, boride, oxide. , inorganic binder and water, and repair is completed through a multi-step curing process using ultra-high temperature ceramic sheets as support materials.

Benefits of technology

Effective repair of large-area damaged coatings is achieved, reducing damage caused by internal stress after drying, improving the oxidation resistance and high temperature resistance of the repaired area, and extending service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116903396B_ABST
    Figure CN116903396B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of anti-oxidation coatings, and specifically relates to an anti-oxidation coating repair material and a method for repairing damaged anti-oxidation coatings. The present invention provides an anti-oxidation coating repair material, comprising a first coating, a second coating and an ultra-high temperature ceramic sheet; the first coating comprises a filler, a first binder and water; the filler is silicon carbide powder and silicon powder or silicon carbide powder; the second coating comprises carbide, boride, oxide, a second binder and water; the carbide is one or more of silicon carbide, zirconium carbide and hafnium carbide, the boride is one or more of zirconium boride, hafnium boride, tantalum boride and titanium boride, and the oxide is one or more of yttrium oxide, aluminum oxide and lanthanum oxide. The repair material provided by the present invention can repair large-area damaged anti-oxidation coatings while ensuring the oxidation resistance of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anti-oxidation coatings, and in particular relates to an anti-oxidation coating repair material and a method for repairing a damaged anti-oxidation coating. Background Art

[0002] Carbon / carbon composites are a new type of composite material with excellent mechanical properties and are widely used in aerospace, military and defense fields. However, the high-temperature oxygen intolerance of carbon / carbon composites hinders their application under ultra-high temperature conditions. Currently, the high-temperature oxidation resistance of carbon / carbon composites is mainly improved by preparing an anti-oxidation coating on the surface of carbon / carbon composites.

[0003] The anti-oxidation coating on the surface of carbon / carbon composite materials is an ultra-high temperature protective coating prepared on the surface of carbon / carbon composite materials, thereby protecting the matrix carbon / carbon composite materials to maintain good mechanical properties in ultra-high temperature aerobic environments. However, in actual application scenarios, the coating may peel off due to improper human operation during the transportation and assembly of parts, or the accumulation of thermal stress due to uneven local heat load under ultra-high temperature service conditions, as well as some other factors, which may cause the ultra-high temperature protective coating to crack or even fall off. After the ultra-high temperature protective coating cracks or falls off, the exposed carbon / carbon composite material will be oxidized and damaged under ultra-high temperature conditions, which will cause damage and affect the service life.

[0004] At present, the problem of damage to ultra-high temperature protective coatings is mainly solved by repairing. For example, Chinese patent CN202110032342.1 discloses a local defect whisker reinforcement repair method and repair coating for carbon / carbon composite material coatings. The method disclosed in this patent can perform on-site instant repair of damaged ultra-high temperature protective coatings, but its repair method is only applicable to damaged coatings with a small area to be repaired. For large-area coating repairs exceeding 20% ​​of the overall coating area, a mixed coating containing a binder and water is used for baking and drying. Due to the shrinkage effect of internal stress, the coating material in the repair area falls off and cracks. Summary of the invention

[0005] In view of this, the present invention provides an anti-oxidation coating repair material and a method for repairing a damaged anti-oxidation coating. The repair method provided by the present invention can repair a large area of ​​damaged anti-oxidation coating with a damaged area exceeding 20%.

[0006] In order to solve the above technical problems, the present invention provides an anti-oxidation coating repair material, which includes a first coating, a second coating and an ultra-high temperature ceramic sheet;

[0007] The first coating comprises a filler, a first binder and water; the filler is silicon carbide powder and silicon powder or silicon carbide powder;

[0008] The second coating includes carbides, borides, oxides, a second binder and water; the carbides are one or more of silicon carbide, zirconium carbide and hafnium carbide, the borides are one or more of zirconium boride, hafnium boride, tantalum boride and titanium boride, and the oxides are one or more of yttrium oxide, aluminum oxide and lanthanum oxide.

[0009] Preferably, the material of the ultra-high temperature ceramic sheet includes ultra-high temperature carbide and / or ultra-high temperature boride.

[0010] Preferably, the ultra-high temperature carbide comprises silicon carbide;

[0011] The ultra-high temperature boride includes one or more of zirconium boride, hafnium boride, tantalum boride, titanium boride and high entropy boride.

[0012] Preferably, the mass ratio of the silicon carbide powder to the silicon powder is 1:0.1-0.5;

[0013] The solid content of the first coating is 50-70%.

[0014] Preferably, the mass ratio of the oxide, carbide and boride is 1:4-10:10-15;

[0015] The solid content of the second coating is 50-80%.

[0016] Preferably, the first binder includes one or more of polycarbosilane, polysilane and modified silane;

[0017] The second binder is an inorganic binder.

[0018] The present invention also provides a method for repairing a damaged anti-oxidation coating using the anti-oxidation coating repair material described in the above technical solution, comprising the following steps:

[0019] The first coating is applied to the damaged surface of the anti-oxidation coating substrate, and then an ultra-high temperature ceramic sheet is adhered thereto, and a first curing is performed to obtain a primary repair coating;

[0020] A second coating is applied on the surface of the primary repair coating, and a second curing is performed to complete the repair of the damaged anti-oxidation coating.

[0021] Preferably, the thickness of the first coating applied is 0.08 to 0.12 mm;

[0022] The temperature of the first curing is 200-300° C., and the time of the first curing is 4-6 minutes.

[0023] Preferably, the second curing includes low-temperature curing and high-temperature curing performed sequentially; the temperature of the low-temperature curing is 20-35°C, and the time of the low-temperature curing is 60-120 minutes; the temperature of the high-temperature curing is 780-820°C, and the time of the high-temperature curing is 0.8-1.2 minutes.

[0024] Preferably, the matrix comprises a carbon / carbon composite material, an aluminum nitride / silicon carbide / carbon fiber epoxy resin composite material or a titanium / zirconium oxide composite material.

[0025] The present invention provides an anti-oxidation coating repair material, comprising a first coating, a second coating and an ultra-high temperature ceramic sheet; the first coating comprises a filler, a first binder and water; the filler is silicon carbide powder and silicon powder or silicon carbide powder; the second coating comprises carbide, boride, oxide, a second binder and water; the carbide is one or more of silicon carbide, zirconium carbide and hafnium carbide, the boride is one or more of zirconium boride, hafnium boride, tantalum boride and titanium boride, and the oxide is one or more of yttrium oxide, aluminum oxide and lanthanum oxide. The present invention uses an ultra-high temperature ceramic sheet with oxidation resistance to divide the damaged large area into multiple small areas. The ultra-high temperature ceramic sheet plays a "skeleton" support role to reduce the damage caused by the internal stress of the coating after drying and curing, and the ultra-high temperature ceramic sheet repair technology can also reduce the amount of coating used, shorten the drying time and speed up the repair speed, and the ultra-high temperature ceramic sheet itself has excellent oxidation resistance, and the repaired damaged area can still maintain good oxidation resistance.

[0026] The present invention provides a method for repairing a damaged anti-oxidation coating using the anti-oxidation coating repair material described in the above technical solution, comprising the following steps: applying a first coating to the surface of a damaged substrate of the anti-oxidation coating, adhering an ultra-high temperature ceramic sheet, performing a first curing, and obtaining a primary repair coating; applying a second coating on the surface of the primary repair coating, performing a second curing, and completing the repair of the damaged anti-oxidation coating. The present invention adheres an ultra-high temperature ceramic sheet of a specific size to the surface of the damaged substrate of the coating under the action of the first coating, which can avoid stress accumulation caused by a large repair area that affects the bonding performance of the repair coating with the substrate; at the same time, the ultra-high temperature ceramic sheet can improve the high temperature resistance and oxidation resistance of the repair coating. The present invention can further improve the compactness of the repair coating and the oxidation resistance under ultra-high temperature conditions by applying a second coating on the surface of the ultra-high temperature ceramic sheet. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic diagram of the structure of the coating obtained by repair in Example 1, wherein the top view is a top view of the primary repair coating, and the cross-sectional view is a schematic diagram of the structure of the longitudinal section of the coating after the repair is completed. DETAILED DESCRIPTION

[0028] The invention provides an anti-oxidation coating repair material, comprising a first coating, a second coating and an ultra-high temperature ceramic sheet.

[0029] In the present invention, the first coating comprises a filler, a first binder and water. In the present invention, the filler is silicon carbide powder and silicon powder or silicon carbide powder. In the present invention, the average particle size of the silicon carbide powder is preferably 100nm to 1μm, more preferably 100nm to 300nm; the average particle size of the silicon powder is preferably 100nm to 500nm, more preferably 100nm to 200nm. In the present invention, when the filler is silicon carbide powder and silicon powder, the mass ratio of the silicon carbide powder to the silicon powder is preferably 1:0.1 to 0.5, more preferably 1:0.1 to 0.25.

[0030] In the present invention, the first binder preferably includes one or more of polycarbosilane, polysilane and modified silane, more preferably polycarbosilane or polysilane, and more preferably polycarbosilane. In the present invention, when the first binder includes two or more of the above-mentioned specific substances, the present invention has no special requirements on the ratio of the specific substances, and any ratio can be used. In the present invention, the mass ratio of the first binder to the filler is preferably 0.5 to 2:100, more preferably 1 to 1.5:100.

[0031] In the present invention, the solid content of the first coating is preferably 50-70%, more preferably 60-65%.

[0032] In the present invention, the filler, the first binder and water are preferably mixed to obtain the first coating. The present invention has no special requirements for the mixing, as long as the mixing is uniform.

[0033] In the present invention, the second coating comprises carbide, boride, oxide, a second binder and water. In the present invention, the carbide is one or more of silicon carbide, zirconium carbide and hafnium carbide, more preferably silicon carbide and / or zirconium carbide. In the present invention, the average particle size of the carbide is preferably 100nm to 500nm, more preferably 100nm to 200nm. In an embodiment of the present invention, the carbide is specifically a mixture of silicon carbide and zirconium carbide in a mass ratio of 7:2, a mixture of silicon carbide and zirconium carbide in a mass ratio of 4:1, or silicon carbide.

[0034] In the present invention, the boride is one or more of zirconium boride, hafnium boride, tantalum boride and titanium boride, preferably one or two of zirconium boride, hafnium boride, tantalum boride and titanium boride. In the present invention, the average particle size of the boride is preferably 100nm to 550nm, more preferably 100nm to 200nm. In an embodiment of the present invention, the boride is specifically a mixture of zirconium boride and hafnium boride in a mass ratio of 5:1, a mixture of zirconium boride and titanium boride in a mass ratio of 1:1, or zirconium boride.

[0035] In the present invention, the oxide is one or more of yttrium oxide, aluminum oxide, and lanthanum oxide, preferably yttrium oxide or aluminum oxide. In the present invention, when the oxide is two or more of the above-mentioned specific substances, the present invention has no special requirements on the ratio of the specific substances, and any ratio can be used. In the present invention, the average particle size of the oxide is preferably 100nm to 500nm, more preferably 100nm to 200nm.

[0036] In the present invention, the mass ratio of the oxide, carbide and boride is preferably 1:4-10:10-15, more preferably 1:8-9:11-12.

[0037] In the present invention, the second binder is preferably an agentless binder, and the inorganic binder preferably includes water glass, cement or clay. In the present invention, the mass ratio of the total mass of the carbide, boride and oxide to the second binder is preferably 100:1.0-3.0, more preferably 100:1.5-2.5.

[0038] In the present invention, the solid content of the second coating is preferably 50-80%, more preferably 50-60%.

[0039] In the present invention, the carbide, boride, oxide, second binder and water are preferably mixed to obtain the second coating. The present invention has no special requirements for the mixing, as long as the mixing is uniform.

[0040] In the present invention, the material of the ultra-high temperature ceramic sheet preferably includes ultra-high temperature carbide and / or ultra-high temperature boride, and is more preferably ultra-high temperature carbide. In the present invention, the ultra-high temperature carbide preferably includes silicon carbide; the ultra-high temperature boride preferably includes one or more of zirconium boride, hafnium boride, tantalum boride, titanium boride and high entropy boride, and is more preferably zirconium boride. The present invention has no special requirements on the source of the ultra-high temperature ceramic sheet, and conventional commercial products can be used.

[0041] The present invention preferably sets the shape and size of the ultra-high temperature ceramic sheet according to the area and shape of the coating to be repaired, so as to ensure that the ultra-high temperature ceramic sheet is closely attached to the damaged substrate of the coating. The present invention can repair the coating damage under complex working conditions by designing the elemental size of the ultra-high temperature ceramic sheet according to the specific situation, and has wide applicability to large-area coating repair of carbon / carbon composite materials.

[0042] The present invention also provides a method for repairing a damaged anti-oxidation coating using the anti-oxidation coating repair material described in the above technical solution, comprising the following steps:

[0043] The first coating is applied to the damaged surface of the anti-oxidation coating substrate, and then an ultra-high temperature ceramic sheet is adhered thereto, and a first curing is performed to obtain a primary repair coating;

[0044] A second coating is applied on the surface of the primary repair coating, and a second curing is performed to complete the repair of the damaged anti-oxidation coating.

[0045] The present invention applies the first coating to the surface of the damaged coating substrate, adheres the ultra-high temperature ceramic sheet, performs the first curing, and obtains the primary repair coating. The present invention preferably pre-treats the damaged coating substrate before applying the first coating; the pre-treatment preferably includes grinding, cleaning and drying in sequence. In the present invention, the substrate preferably includes a carbon / carbon composite material, an aluminum nitride / silicon carbide / carbon fiber epoxy resin composite material or a titanium / zirconium oxide composite material, more preferably a carbon / carbon composite material; the carbon / carbon composite material preferably includes a carbon fiber reinforced carbon-based composite material, a graphite fiber reinforced carbon-based composite material or a ceramic fiber reinforced carbon-based composite material. In the present invention, the damaged coating area preferably accounts for more than 20% of the original coating area, and more preferably 20-30%. In the present invention, the grinding is preferably performed using sandpaper, and the sandpaper is preferably 400# sandpaper. The present invention makes the surface of the damaged coating substrate smooth and flat by grinding, which is conducive to the application of the first coating. In the present invention, the cleaning solvent is preferably alcohol. The present invention has no special requirements for the drying, as long as the surface solvent can be removed.

[0046] In the present invention, the thickness of the first coating is preferably 0.08-0.12 mm, more preferably 0.1 mm. The present invention has no special requirements for the coating, and conventional coating methods in the art can be used.

[0047] In the present invention, the thickness of a single ultra-high temperature ceramic sheet is preferably less than 1 mm, more preferably 0.5-0.8 mm; the area of ​​a single ultra-high temperature ceramic sheet is preferably 5-12% of the coating damage area, more preferably 10%. In the present invention, the shape of the ultra-high temperature ceramic sheet is preferably rectangular, annular or triangular. In the present invention, it is preferred to arrange and adhere in a dot matrix form, and preferably press after adhesion. In the present invention, the spacing between adjacent ultra-high temperature ceramic sheets after arrangement and adhesion is preferably less than 1 cm, more preferably greater than 5 mm and less than 1 cm.

[0048] In the present invention, the temperature of the first curing is preferably 200-300° C., more preferably 200-250° C.; the time of the first curing is preferably 4-6 minutes, more preferably 5 minutes.

[0049] The present invention preferably utilizes a handheld heat gun for the first curing.

[0050] After obtaining the primary repair coating, the present invention applies a second coating on the surface of the primary repair coating, performs a second curing, and completes the repair of the damaged anti-oxidation coating. The present invention preferably applies the second coating in layers, and the thickness of each layer of the second coating is preferably 0.05mm-0.5mm, more preferably 0.05mm-0.2mm, and further preferably 0.08-0.1mm. After each layer of the second coating is applied, it is preferably independently low-temperature cured, and the temperature of the low-temperature curing is preferably 20-35°C, more preferably 25-30°C; the time of the low-temperature curing is preferably 30min-120min, more preferably 60min-120min. After the last layer is coated and low-temperature cured, high-temperature curing is performed, and the temperature of the high-temperature curing is preferably 780-820°C, more preferably 800°C; the time of the high-temperature curing is preferably 0.8-1.2min, more preferably 1min. The present invention reconstructs the phase of high-temperature resistant materials such as silicon carbide inside the anti-oxidation coating through high-temperature curing, and the grains are more tightly bound, which can improve the anti-oxidation performance of the coating.

[0051] The present invention has no special limitation on the number of layers of the second coating, as long as it can be ensured that the repair coating is flush with the surface of the original coating without damage after the second coating is applied.

[0052] The present invention applies the second coating so that the second coating infiltrates the gaps between the ultra-high temperature ceramic sheet elements and the gaps between the ultra-high temperature ceramic sheet and the first coating, thereby improving the density of the repair coating and thus improving the high temperature oxidation resistance of the repair coating.

[0053] The repair method provided by the present invention has low dependence on equipment, a simple repair process, and the coating can generate high-temperature resistant ceramic phase silicon carbide in situ under ultra-high temperature conditions, and is suitable for immediate on-site repair.

[0054] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0055] Example 1

[0056] (1) Cutting the SiC ceramic sheet into square unit sheets with a size of 10*10*0.5 mm to obtain SiC ceramic unit sheets;

[0057] (2) preparing a first coating and a second coating;

[0058] Silicon carbide powder with an average particle size of 200 nm and silicon powder with an average particle size of 200 nm are mixed with a polycarbosilane binder and water in a mass ratio of 2:1 to obtain a first coating with a solid content of 65% as an inner coating; the amount of polycarbosilane added is 0.8wt% of the total mass of the silicon carbide powder and the silicon powder;

[0059] A mixture of yttrium oxide powder (average particle size of 100 nm), zirconium carbide powder (average particle size of 100 nm), silicon carbide powder (average particle size of 200 nm) and zirconium boride powder (average particle size of 100 nm) in a mass ratio of 1:2:8:11 is used as a filler, water glass is used as a second binder (the mass ratio of the total mass of yttrium oxide powder, zirconium carbide powder and silicon carbide powder to the second binder is 100:2), the filler, the second binder and water are mixed to obtain a second coating with a solid content of 50% as an outer coating;

[0060] (3) Using 400# sandpaper, the damaged coating on the surface of the carbon fiber / carbon matrix composite material, whose damaged area accounts for 20% of the original coating area, is polished until the surface is smooth and flat, and then cleaned with alcohol and dried for processing;

[0061] (4) After applying a coating with a thickness of 0.1 mm on the pretreated substrate surface using the first coating, SiC ceramic element sheets are arranged in a lattice form (the spacing between adjacent SiC ceramic element sheets is 60 mm) and adhered to the coating surface and pressed tightly, and then heated and cured at 200° C. for 5 min using a handheld hot air gun to obtain a primary repair coating;

[0062] (5) using the second coating to fill the surface of the primary repair coating in a pit-filling manner, so that the second coating infiltrates the gaps between the silicon carbide ceramic element sheets and the gaps between the coatings formed by the silicon carbide ceramic element sheets and the first coating, and curing at room temperature at 25° C. for 60 minutes to obtain a coating with a thickness of 0.2 mm;

[0063] (6) Apply a second coating on the obtained coating surface and then cure it at room temperature. Repeat the steps of coating and curing at room temperature for 6 times, then use a butane spray gun to treat the coating surface at 800° C. for 1 min to complete the repair.

[0064] The total thickness of the repair coating is 0.7 mm. The repaired coating is tightly bonded to the silicon carbide wafer, carbon fiber / carbon matrix composite material, and the original coating without cracks. The density of the repaired coating is ≥1.90 g / cm 3 , compressive strength ≥ 150MPa, static oxidation resistance test at 1500℃ for 2h in air atmosphere in a tube furnace, the oxide layer thickness of the sample after repair coating is 10mm, and the oxide layer thickness of the blank control sample (other areas without damage to the coating before repair) is 18mm.

[0065] Figure 1 It is a schematic diagram of the structure of the coating obtained by repair in Example 1, wherein the top view is a top view of the primary repair coating, and the cross-sectional view is a schematic diagram of the structure of the longitudinal section of the coating after the repair is completed.

[0066] Example 2

[0067] (1) Cutting the SiC ceramic sheet into regular triangle unit sheets with a size of 10*10*10*0.3 mm to obtain SiC ceramic unit sheets;

[0068] (2) preparing a first coating and a second coating;

[0069] Silicon carbide powder with an average particle size of 200 nm is mixed with a polycarbosilane binder and water to obtain a first coating with a solid content of 50% as an inner coating; the amount of polycarbosilane added is 0.8wt% of the mass of the silicon carbide powder;

[0070] A mixture of aluminum oxide powder (average particle size of 100 nm), silicon carbide powder (average particle size of 200 nm), zirconium boride powder (average particle size of 100 nm) and titanium boride powder (average particle size of 100 nm) in a mass ratio of 1:8:6:6 is used as a filler, clay is used as a second binder (the mass ratio of the total mass of aluminum oxide powder, silicon carbide powder and zirconium boride powder to the second binder is 100:2), the filler, the second binder and water are mixed to obtain a second coating with a solid content of 50% as an outer coating;

[0071] (3) Using 400# sandpaper, the damaged coating on the surface of the carbon fiber / carbon matrix composite material, whose damaged area accounts for 20% of the original coating area, is polished until the surface is smooth and flat, and then cleaned with alcohol and dried for processing;

[0072] (4) After applying a coating with a thickness of 0.1 mm on the pretreated substrate surface using the first coating, SiC ceramic element sheets are arranged in a lattice form (the spacing between adjacent SiC ceramic element sheets is 70 mm) and adhered to the coating surface and pressed tightly, and then heated and cured at 200° C. for 5 min using a handheld hot air gun to obtain a primary repair coating;

[0073] (5) using the second coating to fill the surface of the primary repair coating in a pit-filling manner, so that the second coating infiltrates the gaps between the silicon carbide ceramic element sheets and the gaps between the coatings formed by the silicon carbide ceramic element sheets and the first coating, and curing at room temperature at 25° C. for 60 minutes to obtain a coating with a thickness of 0.1 mm;

[0074] (6) Apply a second coating on the obtained coating surface and then cure it at room temperature. Repeat the steps of coating and curing at room temperature for 5 times, then treat the coating surface with a butane spray gun at 800° C. for 1 min to complete the repair.

[0075] The total thickness of the repair coating is 0.6 mm. The repaired coating is tightly bonded to the silicon carbide wafer, carbon fiber / carbon matrix composite material, and the original coating without cracks. The density of the repaired coating is ≥1.80 g / cm 3 , compressive strength ≥160MPa, static oxidation resistance test at 1500℃ for 2h in air atmosphere in a tube furnace, the oxide layer thickness of the sample after repair coating is 12.5mm, and the oxide layer thickness of the blank control sample (other areas without damage to the coating before repair) is 18mm.

[0076] Example 3

[0077] (1) cutting a ZrB2-SiC ceramic sheet (the volume percentage of SiC in the ceramic sheet is 20 vol%) into regular triangle elementary sheets with a size of 10*10*0.3 mm to obtain a ZrB2-SiC ceramic elementary sheet;

[0078] (2) preparing a first coating and a second coating;

[0079] Silicon carbide powder with an average particle size of 200 nm and silicon powder with an average particle size of 200 nm are mixed with a polycarbosilane binder and water in a mass ratio of 8:1 to obtain a first coating with a solid content of 50% as an inner coating; the amount of polycarbosilane added is 0.8wt% of the total mass of the silicon carbide powder and the silicon powder;

[0080] A mixture of yttrium oxide powder (average particle size of 100 nm), silicon carbide powder (average particle size of 200 nm), zirconium boride powder (average particle size of 100 nm) and titanium boride powder (average particle size of 100 nm) in a mass ratio of 1:8:6:6 is used as a filler, clay is used as a second binder (the total mass of yttrium oxide powder, silicon carbide powder, zirconium boride powder and titanium boride powder and the mass ratio of the second binder is 100:2), the filler, the second binder and water are mixed to obtain a second coating with a solid content of 50% as an outer coating;

[0081] (3) Using 400# sandpaper, the damaged coating on the surface of the carbon fiber / carbon matrix composite material, whose damaged area accounts for 20% of the original coating area, is polished until the surface is smooth and flat, and then cleaned with alcohol and dried for processing;

[0082] (4) After applying a coating with a thickness of 0.1 mm on the pretreated substrate surface using the first coating, ZrB2-SiC ceramic element sheets are arranged in a lattice form (the spacing between adjacent SiC ceramic element sheets is 55 mm) and adhered to the coating surface and pressed tightly, and then heated and cured at 200° C. for 5 min using a handheld hot air gun to obtain a primary repair coating;

[0083] (5) applying a second coating to the surface of the primary repair coating in a filling manner, so that the second coating penetrates the gaps between the ZrB2-SiC ceramic element sheets and the gaps between the ZrB2-SiC ceramic element sheets and the coatings formed by the first coating, and curing at room temperature at 25° C. for 60 minutes to obtain a coating with a thickness of 0.2 mm;

[0084] (6) Apply a second coating on the obtained coating surface and then cure it at room temperature. Repeat the steps of coating and curing at room temperature four times, then treat the coating surface with a butane spray gun at 800° C. for 1 min to complete the repair.

[0085] The total thickness of the repair coating is 0.5mm. The repaired coating is tightly bonded to the ceramic sheet element, carbon fiber / carbon matrix composite material, and the original coating without cracks. The density of the repair coating is ≥1.60g / cm 3 , compressive strength ≥145MPa, static oxidation resistance test at 1500℃ for 2h in air atmosphere in a tube furnace, the oxide layer thickness of the sample after repair coating is 10.4mm, and the oxide layer thickness of the blank control sample (other areas without damage to the coating before repair) is 18mm.

[0086] Example 4

[0087] (1) Cutting the ZrB2 ceramic sheet into square elementary sheets with a size of 10*10*10*0.3 mm to obtain ZrB2 ceramic elementary sheets;

[0088] (2) preparing a first coating and a second coating;

[0089] Silicon carbide powder with an average particle size of 200 nm and silicon powder with an average particle size of 200 nm are mixed with a polycarbosilane binder and water in a mass ratio of 9:1 to obtain a first coating with a solid content of 60% as an inner coating; the amount of polycarbosilane added is 0.8wt% of the total mass of the silicon carbide powder and the silicon powder;

[0090] A mixture of yttrium oxide powder (average particle size of 100 nm), silicon carbide powder (average particle size of 200 nm), zirconium boride powder (average particle size of 100 nm) and hafnium boride powder (average particle size of 100 nm) in a mass ratio of 1:8:10:2 is used as a filler, clay is used as a second binder (the total mass of yttrium oxide powder, silicon carbide powder, zirconium boride powder and hafnium boride powder and the mass ratio of the second binder is 100:2), the filler, the second binder and water are mixed to obtain a second coating with a solid content of 60% as an outer coating;

[0091] (3) Using 400# sandpaper, the damaged coating on the surface of the carbon fiber / carbon matrix composite material, whose damaged area accounts for 20% of the original coating area, is polished until the surface is smooth and flat, and then cleaned with alcohol and dried for processing;

[0092] (4) After applying a coating with a thickness of 0.1 mm on the pretreated substrate surface using the first coating, ZrB2 ceramic element sheets are arranged in a lattice form (the spacing between adjacent SiC ceramic element sheets is 65 mm) and adhered to the coating surface and pressed tightly, and then heated and cured at 200° C. for 5 min using a handheld hot air gun to obtain a primary repair coating;

[0093] (5) using a second coating to fill the surface of the primary repair coating, so that the second coating penetrates the gaps between the boride zirconium ceramic element sheets and the gaps between the coatings formed by the boride zirconium ceramic element sheets and the first coating, and curing at room temperature for 80 minutes at 25° C. to obtain a coating with a thickness of 0.1 mm;

[0094] (6) Apply a second coating on the obtained coating surface and then cure it at room temperature. Repeat the steps of coating and curing at room temperature three times, then use a butane spray gun to treat the coating surface at 800° C. for 1 min to complete the repair.

[0095] The total thickness of the repair coating is 0.4 mm. The repaired coating is tightly bonded to the zirconium boride ceramic sheet, carbon fiber / carbon matrix composite material, and the original coating without cracks. The density of the repaired coating is ≥1.70 g / cm 3 , compressive strength ≥148MPa, static oxidation resistance test at 1500℃ for 2h in air atmosphere in a tube furnace, the oxide layer thickness of the sample after repair coating is 12.6mm, and the oxide layer thickness of the blank control sample (other areas without damage to the coating before repair) is 18mm.

[0096] Example 5

[0097] (1) Cutting the SiC ceramic sheet into square unit sheets with a size of 10*10*10*0.3 mm to obtain SiC ceramic unit sheets;

[0098] (2) preparing a first coating and a second coating;

[0099] Silicon carbide powder with an average particle size of 200 nm is mixed with a polycarbosilane binder and water to obtain a first coating with a solid content of 60% as an inner coating; the amount of polycarbosilane added is 0.8wt% of the mass of the silicon carbide powder;

[0100] A mixture of lanthanum oxide powder (average particle size of 100 nm), silicon carbide powder (average particle size of 200 nm), zirconium carbide powder (average particle size of 100 nm) and zirconium boride powder (average particle size of 100 nm) in a mass ratio of 1:7:2:12 is used as a filler, clay is used as a second binder (the total mass of lanthanum oxide powder, silicon carbide powder, zirconium carbide and zirconium boride powder and the mass ratio of the second binder are 100:2), the filler, the second binder and water are mixed to obtain a second coating with a solid content of 50% as an outer coating;

[0101] (3) Using 400# sandpaper, the damaged coating on the surface of the carbon fiber / carbon matrix composite material, whose damaged area accounts for 20% of the original coating area, is polished until the surface is smooth and flat, and then cleaned with alcohol and dried for processing;

[0102] (4) After applying a coating with a thickness of 0.1 mm on the pretreated substrate surface using the first coating, SiC ceramic element sheets are arranged in a lattice form (the spacing between adjacent SiC ceramic element sheets is 58 mm) and adhered to the coating surface and pressed tightly, and then heated and cured at 200° C. for 5 min using a handheld hot air gun to obtain a primary repair coating;

[0103] (5) using the second coating to fill the surface of the primary repair coating, so that the second coating penetrates the gaps between the silicon carbide ceramic element sheets and the gaps between the coatings formed by the silicon carbide ceramic element sheets and the first coating, and curing at room temperature at 25° C. for 80 minutes to obtain a coating with a thickness of 0.1 mm;

[0104] (6) Apply a second coating on the obtained coating surface and then cure it at room temperature. Repeat the steps of coating and curing at room temperature three times, then use a butane spray gun to treat the coating surface at 800° C. for 1 min to complete the repair.

[0105] The total thickness of the repair coating is 0.4 mm. The repaired coating is tightly bonded to the silicon carbide wafer, carbon fiber / carbon matrix composite material, and the original coating without cracks. The density of the repaired coating is ≥1.70 g / cm 3 , compressive strength ≥150MPa, static oxidation resistance test at 1500℃ for 2h in air atmosphere in a tube furnace, the oxide layer thickness of the sample after repair coating is 11.2mm, and the oxide layer thickness of the blank control sample (other areas without damage to the coating before repair) is 18mm.

[0106] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. An anti-oxidation coating repair material, characterized in that: It includes a first coating, a second coating and an ultra-high temperature ceramic sheet; The first coating comprises a filler, a first binder and water; the filler is a mixture of silicon carbide powder and silicon powder or silicon carbide powder; the first binder comprises one or more of polycarbosilane, polysilane and modified silane; The second coating comprises carbide, boride, oxide, a second binder and water; the carbide is one or more of silicon carbide, zirconium carbide and hafnium carbide, the boride is one or more of zirconium boride, hafnium boride, tantalum boride and titanium boride, the oxide is one or more of yttrium oxide, aluminum oxide and lanthanum oxide; the second binder is an inorganic binder. When the anti-oxidation coating repair material is used for repair, the first coating is first applied, then the ultra-high temperature ceramic sheet is attached, and finally the second coating is applied.

2. The anti-oxidation coating repair material according to claim 1, characterized in that: The material of the ultra-high temperature ceramic sheet includes ultra-high temperature carbide and / or ultra-high temperature boride.

3. The anti-oxidation coating repair material according to claim 2, characterized in that: The ultra-high temperature carbide includes silicon carbide; The ultra-high temperature boride includes one or more of zirconium boride, hafnium boride, tantalum boride, titanium boride and high entropy boride.

4. The anti-oxidation coating repair material according to claim 1, characterized in that: The mass ratio of the silicon carbide powder to the silicon powder is 1:0.1-0.5; The solid content of the first coating is 50-70%.

5. The anti-oxidation coating repair material according to claim 1, characterized in that: The mass ratio of the oxide, carbide and boride is 1:4-10:10-15; The solid content of the second coating is 50-80%.

6. A method for repairing a damaged anti-oxidation coating using the anti-oxidation coating repair material according to any one of claims 1 to 5, comprising the following steps: The first coating is applied to the damaged surface of the anti-oxidation coating, and then an ultra-high temperature ceramic sheet is adhered to the surface, and a first curing is performed to obtain a primary repair coating; A second coating is applied on the surface of the primary repair coating, and a second curing is performed to complete the repair of the damaged anti-oxidation coating.

7. The method for repairing a damaged anti-oxidation coating using an anti-oxidation coating repair material according to claim 6, characterized in that: The thickness of the first coating is 0.08-0.12 mm; The temperature of the first curing is 200-300° C., and the time of the first curing is 4-6 minutes.

8. The method for repairing a damaged anti-oxidation coating using an anti-oxidation coating repair material according to claim 6, characterized in that: The second curing includes low temperature curing and high temperature curing performed sequentially; the temperature of the low temperature curing is 20~35°C, and the time of the low temperature curing is 60~120min; the temperature of the high temperature curing is 780~820°C, and the time of the high temperature curing is 0.8~1.2min.

9. The method for repairing a damaged anti-oxidation coating using an anti-oxidation coating repair material according to claim 6, characterized in that: The matrix includes a carbon / carbon composite material, an aluminum nitride / silicon carbide / carbon fiber epoxy resin composite material or a titanium / zirconium oxide composite material.

Citation Information

Patent Citations

  • Whisker reinforced repairing method for local defects of carbon / carbon composite material coating and repairing coating

    CN112745146A

  • Repairing method of ceramic-based composite material coating with utilization temperature of being more than or equal to 1400 DEG C

    CN102757260A

  • Method for repairing thermal protection coating of silicon carbide ceramic matrix composite component

    CN111039698A

  • Thermal protection material structure damage repair patch and preparation and use methods thereof

    CN111517795A

  • Automobile body corrosion perforation repair process

    CN115350885A