A method for preparing highly dispersed white carbon black

By adding imidazole dispersant to the reaction of fluosiliic acid and ammonia, the problem of poor dispersion of white carbon black in rubber is solved, the compatibility and performance of white carbon black and rubber is improved, and high dispersibility white carbon black is achieved The preparation of the tire industry is suitable for the tire industry and simplifies the process and reduces costs.

CN117023596BActive Publication Date: 2024-12-06HENAN FLUORINE BASED NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311067706.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-23
Publication Date
2024-12-06
Estimated Expiration
2043-08-23

AI Technical Summary

Technical Problem

In the prior art, white carbon black prepared with fluosiliic acid as the silicon source has poor dispersion in rubber, resulting in the inability to be effectively applied to the tire industry.

Method used

Imidazole dispersant is added during the reaction of fluorosiliic acid and ammonia water, and the ionic liquid is formed by coordination with the free fluorine ions in the system, reducing the free fluorine concentration on the surface of the white carbon black, and improving the white carbon black and the white carbon black through in-situ modification. Rubber compatibility.

Benefits of technology

The preparation of high dispersible white carbon black is achieved, which improves the tensile strength and tear-break elongation performance of rubber. It is suitable for rubber tire field, simplifies the process, reduces costs, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a method for preparing highly dispersed white carbon black, belonging to the technical field of powder material preparation. The method for preparing highly dispersed white carbon black of the present invention comprises the following steps: adding an imidazole dispersant during the reaction of fluorosilicic acid and ammonia water, and obtaining highly dispersed white carbon black after solid-liquid separation and drying after the reaction. The white carbon black prepared by the present invention has low free fluorine content, low polarity, good dispersibility, good compatibility with rubber, and has high tensile strength and elongation at break after combining with rubber, and is suitable for the field of rubber tires. In addition, in the preparation process, fluorine is directly removed and white carbon black is modified in situ at the same time, the process is simple, the cost is low, and it is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder material preparation, and particularly relates to a method for preparing highly dispersed white carbon black. Background Art

[0002] White carbon black is also known as hydrated silicon dioxide, with a molecular formula of SiO2·nH2O. Due to its good chemical stability, electrical insulation and high specific surface area, it is widely used in more than a dozen fields such as plastics, rubber, papermaking, coatings, dyes and inks. The commonly used synthesis methods of white carbon black are divided into gas phase method and precipitation method. Due to its significant cost advantage, the precipitation method is currently the focus of domestic and foreign scholars and industry.

[0003] The traditional mainstream precipitation process (Na2SiO3+2H + =SiO2·nH2O+2Na + +H2O) is made of sodium silicate (Na2SiO3) as raw material, using hydrochloric acid or sulfuric acid to react, and obtaining white carbon black through precipitation, filtration, washing, drying and calcination under certain temperature, time and pressure conditions. In addition, due to its lower cost advantage, the process of synthesizing white carbon black using cheap fluorosilicic acid as a byproduct of phosphate fertilizer as raw material (H2SiF6+6NH4OH=6NH4F+SiO2·nH2O, n=4) has attracted much attention. However, in this process, since white carbon black is produced by precipitation in the liquid phase, the hydroxyl groups on its surface will promote the aggregation of white carbon black. More importantly, there will be 0.1~0.5g / L of trace free fluorine (ammonium fluoride) in the structure of separated white carbon black. Since fluorine has a strong polarity and poor compatibility with polymer rubber, it is impossible to obtain high dispersion performance for application in the tire industry.

[0004] According to prior art reports, free fluorine in powder materials can be removed by multiple washing, ion exchange, and plasma treatment. Although these methods can remove trace fluorine in the structure of powder materials, they are all post-processing methods with high costs and cannot be applied in large-scale production. Therefore, there is an urgent need for a preparation method that removes free fluorine during the preparation process and improves the dispersibility of white carbon black. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing highly dispersible white carbon black, so as to solve the problem that the white carbon black prepared with fluorosilicic acid as a silicon source has poor dispersibility in rubber.

[0006] To achieve the above object, the technical solution of the method for preparing highly dispersible white carbon black of the present invention is:

[0007] A method for preparing highly dispersed white carbon black comprises the following steps: adding an imidazole dispersant during the reaction of fluorosilicic acid and ammonia water, and performing solid-liquid separation and drying after the reaction to obtain highly dispersed white carbon black.

[0008] The method for preparing highly dispersible white carbon black provided by the present invention comprises the following steps: introducing an imidazole dispersant to coordinate with free fluorine ions in the system to form an ionic liquid, thereby reducing the free fluorine concentration on the surface of the white carbon black, thereby reducing the polarity and improving the dispersibility of the white carbon black; and the imidazole dispersant can promote the fusion of the white carbon black and the rubber by in-situ modification of the white carbon black during the preparation process, thereby enhancing the interface interaction between the white carbon black and the rubber, and improving the compatibility between the white carbon black and the rubber, thereby improving the tensile strength and elongation at break performance of the rubber.

[0009] The white carbon black obtained by the present invention has a specific surface area of ​​150 to 300 m 2 / g, oil absorption value 2.4~3.2cm 3 / g. The tensile strength is 25-35MPa and the elongation at break is 500-800%. It can be used in the field of rubber tires, meets the requirements for the preparation of highly dispersed silica and develops a new production process for silica.

[0010] The method for preparing highly dispersed white carbon black provided by the present invention directly removes fluorine and simultaneously in-situ modifies the white carbon black during the preparation process, does not require a post-treatment defluorination process, has a simple process, low cost, and is suitable for large-scale production.

[0011] In order to enrich the pore structure of white carbon black and improve the coordination ability of the imidazole dispersant with free fluorine, preferably, the imidazole dispersant is selected from one or more of 2-methylimidazole, 2-ethyl-4-methylimidazole and diphenylimidazole.

[0012] In order to effectively reduce the content of free fluorine in white carbon black, preferably, the amount of the imidazole dispersant added is 0.5wt.% to 40wt.% of the theoretical designed white carbon black product mass.

[0013] In order to completely react fluorosilicic acid and aqueous ammonia, preferably, the reaction temperature is 10 to 95°C.

[0014] When the pH value of the system is greater than 8, since the precipitate generated in the system is nano-oxide, it is easy to agglomerate. At this time, the dispersing effect of the imidazole dispersant is relatively poor, and the modification effect on silica is not good. In order to improve the dispersing efficiency of the dispersant and at the same time improve the modification effect of the imidazole dispersant on silica, preferably, the reaction is to gradually add ammonia water to fluorosilicic acid, monitor the system pH during the reaction, and when the system pH reaches 6 to 8, add the imidazole dispersant, and then age.

[0015] The purpose of aging is to fully dissociate the imidazole dispersant and retain it in the surface structure of partially synthesized white carbon black. In order to ensure that the system is fully mixed after the imidazole dispersant is added, preferably, the aging time is 0.1 to 3 hours.

[0016] In order to increase the reaction rate, preferably, the concentration of the fluorosilicic acid is 10-35%, and the concentration of the ammonia water is 1-20 mol / L.

[0017] In order to mix the materials evenly and increase the reaction speed, the ammonia water is stirred simultaneously when being added, and the stirring speed is 50-500r / min.

[0018] In order to further reduce the residual fluoride ion content on the surface of white carbon black, preferably, after the aging, ammonia water is continuously added to react to the end point. The ammonia water added after aging reacts with the mixture to form an ionic liquid to reduce the residual fluoride ion on the surface of white carbon black.

[0019] Preferably, the pH of the system is monitored during the process of continuing to add ammonia water, and the reaction is completed when the pH of the system is 8.1-9.

[0020] In order to fully disperse part of the white carbon black, control the primary crystal size and pore structure of the white carbon black, and avoid agglomeration, preferably, stirring is continued after the aging, and the stirring speed is 300-800 r / min. DETAILED DESCRIPTION

[0021] A method for preparing highly dispersed white carbon black comprises the following steps: adding an imidazole dispersant during the reaction of fluorosilicic acid and ammonia water, and performing solid-liquid separation and drying after the reaction to obtain highly dispersed white carbon black.

[0022] In a specific embodiment, the theoretical molar ratio of fluorosilicic acid to ammonia water is 1:6. Since ammonia water is volatile, the amount of ammonia water added is excessive according to the theoretical molar ratio of fluorosilicic acid to ammonia water.

[0023] In a specific embodiment, the initial pH of fluorosilicic acid is between 1.5 and 2.5, and the addition of ammonia water will increase the pH of the system. When the pH reaches between 6 and 8, white carbon black particles will be formed. At this time, the imidazole dispersant is introduced and fully mixed with it. When the imidazole dispersant is added, the addition of ammonia water is stopped. If ammonia water is continued to be added, it will immediately react with the imidazole dispersant to form a flocculated precipitate.

[0024] In a specific embodiment, the ammonia water is gradually added to the fluosilicic acid. The ammonia water can be added to the fluosilicic acid by dropwise addition. In order to ensure sufficient contact between the raw materials during the dropwise addition, preferably, the ammonia water dropping speed is 1 to 20 g / min. It can also be that a portion of the ammonia water is reacted with the fluosilicic acid in a microchannel reactor by calculation to make its pH value 6 to 8, an imidazole dispersant is added for aging, and then another portion of the ammonia water and the above-mentioned aged reactants are added to the microchannel reactor to continue the reaction until the pH value is 8.1 to 9, reaching the reaction endpoint.

[0025] In a specific implementation manner, the drying temperature is 100-150° C., and the drying time is 2-6 hours.

[0026] The technical solution of the present invention is further described below in conjunction with specific embodiments. The chemical reagents involved in the following embodiments are all commercially available conventional products unless otherwise specified.

[0027] 1. Specific embodiment of the method for preparing highly dispersible white carbon black of the present invention

[0028] Example 1

[0029] In this embodiment, highly dispersed white carbon black is prepared using fluorosilicic acid as a raw material. According to the stoichiometric formula of H2SiF6+6NH4OH=6NH4F+SiO2·nH2O, n=4, the theoretically designed prepared white carbon black product is 100g, and the preparation process includes the following steps:

[0030] 1091g of 10% fluorosilicic acid solution was taken as the base liquid, and 2mol / L ammonia solution was added to the base liquid for reaction. The reaction temperature was 20°C, the ammonia solution was added at a rate of 1g / min, stirring was started at the same time, and the stirring speed was 200r / min. The pH of the system was monitored during the reaction. When the pH of the system reached 8, the addition of ammonia solution was stopped, 20g of dispersant dimethylimidazole (2MI) was added, stirring was stopped after uniform mixing, and aging was performed for 1h. After aging, high-speed stirring was performed again at a stirring rate of 800r / min, and ammonia solution was continued to be added dropwise at 20°C until the reaction reached the end point. The pH value of the reaction end point was 9; the concentration of 2mol / L ammonia solution added during the entire reaction process was 2485g (2322mL). After the reaction was completed, 98g of white carbon black product was obtained by suction filtration, filter cake washing, and drying at 120°C for 3h. The specific surface area of ​​the white carbon black product was 195m 2 / g, oil absorption value 2.9cm 3 / g.

[0031] Example 2

[0032] 1091g of 10% fluorosilicic acid solution was taken as the base liquid, and 2mol / L ammonia solution was added to the base liquid for reaction. The reaction temperature was 20°C, the ammonia solution was added at a rate of 1g / min, stirring was started at the same time, and the stirring speed was 200r / min. The pH of the system was monitored during the reaction. When the pH of the system reached 8, the addition of ammonia solution was stopped, 20g of dispersant 2-ethyl-4-methylimidazole was added, stirring was stopped after uniform mixing, and aging was performed for 1h. After aging, high-speed stirring was performed again at a stirring rate of 800r / min, and ammonia solution was continued to be added dropwise at 20°C until the reaction reached the end point. The pH value of the reaction end point was 9; the concentration of 2mol / L ammonia solution added during the entire reaction process was 2485g (2322mL). After the reaction was completed, 98g of white carbon black product was obtained by suction filtration, filter cake washing, and drying at 120°C for 3h. The specific surface area of ​​the white carbon black product was 170m 2 / g, oil absorption value 2.7cm 3 / g.

[0033] Example 3

[0034] 1091g of 10% fluorosilicic acid solution was taken as the base liquid, and 2mol / L ammonia solution was added to the base liquid for reaction. The reaction temperature was 20°C, the ammonia solution was added at a rate of 1g / min, and stirring was started at the same time. The stirring speed was 200r / min. The pH of the system was monitored during the reaction. When the pH of the system reached 8, the addition of ammonia solution was stopped, 20g of dispersant diphenylimidazole and 10g of dispersant dimethylimidazole (2MI) were added, and stirring was stopped after uniform mixing. The mixture was aged for 1h, and then stirred at a high speed again after aging. The stirring speed was 800r / min, and ammonia solution was continued to be added dropwise at 20°C until the reaction reached the end point. The pH value of the reaction end point was 9. The concentration of 2mol / L ammonia solution added during the entire reaction process was 2485g (2322mL). After the reaction, 98g of white carbon black product was obtained by suction filtration, filter cake washing, and drying at 120°C for 3h. The specific surface area of ​​the white carbon black product was 220m 2 / g, oil absorption value 3.1cm 3 / g.

[0035] Example 4

[0036] 311.7g of 35% fluorosilicic acid solution was taken as the base liquid, and 2mol / L ammonia solution was added to the base liquid for reaction. The reaction temperature was 95°C, the ammonia solution was added at a rate of 20g / min, and stirring was started at the same time. The stirring speed was 50r / min. The pH of the system was monitored during the reaction. When the pH of the system reached 6, the addition of ammonia solution was stopped, 40g of dispersant diphenylimidazole was added, stirring was stopped after uniform mixing, and aging was performed for 0.1h. After aging, high-speed stirring was performed again at a stirring speed of 300r / min. At the same time, ammonia solution was continued to be added dropwise at 95°C until the reaction reached the end point. The pH value of the reaction end point was 9; the concentration of 2mol / L ammonia solution added during the entire reaction process was 2485g (2322mL). After the reaction, 98g of white carbon black product was obtained by suction filtration, filter cake washing, and drying at 120°C for 3h. The specific surface area of ​​the white carbon black product was 193m 2 / g, oil absorption value 2.5cm 3 / g.

[0037] Example 5

[0038] 311.7g of 35% fluorosilicic acid solution was taken as the base liquid, and 20mol / L ammonia solution was added to the base liquid for reaction. The reaction temperature was 10°C, the ammonia solution was added at a rate of 1g / min, stirring was started at the same time, and the stirring speed was 500r / min. The pH of the system was monitored during the reaction. When the pH of the system reached 8, the addition of ammonia solution was stopped, 0.5g of dispersant 2-ethyl-4-methylimidazole was added, stirring was stopped after uniform mixing, and aging was carried out for 3h. After aging, high-speed stirring was carried out again, and the stirring speed was 800r / min. At the same time, ammonia solution was continued to be added dropwise at 10°C until the reaction reached the end point. The pH value of the reaction end point was 9; the concentration of 20mol / L ammonia solution added dropwise during the entire reaction process was 395g (233mL). After the reaction was completed, 98g of white carbon black product was obtained by suction filtration, filter cake washing, and drying at 150°C for 6h. The specific surface area of ​​the white carbon black product was 290m 2 / g, oil absorption value 3.0cm 3 / g.

[0039] Example 6

[0040] 1100g of 10% fluorosilicic acid solution and 1988g of 2mol / L ammonia solution were placed in beakers respectively. The two reactants were simultaneously pumped into the microchannel reactor through two peristaltic pumps. The pH at the outlet of the microchannel reactor was detected to be 8, and the reaction temperature was 40°C. The intermediate product was stored in a beaker and 20g of dispersant diphenylimidazole was added. After stirring until uniform mixing, aging for 1h, the intermediate product containing diphenylimidazole and 497g of 2mol / L ammonia solution were simultaneously pumped into the microchannel reactor through two peristaltic pumps. The pH at the outlet of the microchannel reactor was detected to be 9, and the reaction temperature was 50°C. The concentration of 2mol / L ammonia solution used in the whole reaction process was 2485g (2322mL). After the reaction was completed, 98g of white carbon black product was obtained by filtration, filter cake washing, and drying at 120°C for 3h. The specific surface area of ​​the white carbon black product was 270m 2 / g, oil absorption value 2.8cm 3 / g.

[0041] Example 7

[0042] 311.7 g of 35% fluorosilicic acid solution and 160 g of 20 mol / L ammonia solution were placed in beakers respectively. The two reactants were simultaneously pumped into the microchannel reactor through two peristaltic pumps. The pH at the outlet of the microchannel reactor was detected to be 6, and the reaction temperature was 60°C. The intermediate product was stored in a beaker and 20 g of dispersant diphenylimidazole and 20 g of dispersant 2-methylimidazole were added. After stirring until uniformly mixed, the mixture was aged for 3 h. The intermediate product containing diphenylimidazole and 235 g of 20 mol / L ammonia solution were simultaneously pumped into the microchannel reactor through two peristaltic pumps. The pH at the outlet of the microchannel reactor was detected to be 8.5, and the reaction temperature was 70°C. The concentration of 20 mol / L ammonia solution used in the whole reaction process was 395 g (233 mL). After the reaction was completed, 98 g of white carbon product was obtained by filtration, filter cake washing, and drying at 100°C for 6 h. The specific surface area of ​​the white carbon product was 160 m 2 / g, oil absorption value 3.1cm 3 / g.

[0043] 2. Comparison

[0044] This comparative example uses fluorosilicic acid as a raw material to prepare highly dispersed white carbon black. The difference from Example 1 is that no dispersant dimethylimidazole is introduced. The preparation process includes the following steps:

[0045] 1100g of 10% fluorosilicic acid solution was taken as the base liquid, and 2mol / L ammonia solution was added to the base liquid for reaction. The reaction temperature was 20°C, the ammonia solution was added at a rate of 1g / min, stirring was started at the same time, and the stirring rate was 200r / min. The pH of the system was monitored during the reaction. When the pH of the system reached 8, the dispersant dimethylimidazole was not introduced, and the ammonia solution was continued to be added at 20°C until the reaction reached the end point. The pH value at the end point of the reaction was 9. The concentration of 2mol / L ammonia solution added during the entire reaction process was 1360g (1000mL). After the reaction was completed, 98g of white carbon black product was obtained by suction filtration, filter cake washing, and drying at 120°C for 3h. The specific surface area of ​​the white carbon black product was 135m 2 / g, oil absorption value 2.1cm 3 / g.

[0046] 3. Experimental Examples

[0047] Experimental example

[0048] In this experimental example, raw materials such as white carbon black, rubber, and modifiers are prepared into rubber products through processes such as internal mixing, open mixing, and vulcanization, and the tensile strength and elongation at break of the rubber products are tested. The tensile strength and elongation at break are tested using a tensile testing machine. The test results of the tensile strength and elongation at break of the rubber products made of white carbon black in the embodiments and comparative examples are shown in Table 1.

[0049] Table 1 Tensile strength and elongation at break of rubber products

[0050] Tensile strength(MPa) Elongation at break (%) Example 1 35 700 Example 2 30 620 Example 3 32 720 Example 4 26 610 Example 5 32 645 Example 6 28 590 Example 7 27 575 Comparative Example 25 500

[0051] It can be seen from Table 1 that the tensile strength and elongation at break of the rubber product made of the highly dispersible silica provided by the present invention are higher than those of the comparative example, indicating that the addition of the imidazole dispersant can improve the dispersibility of silica in the rubber.

Claims

1. A method for preparing highly dispersed white carbon black, It is characterized in that The following steps are involved: An imidazole dispersant is added during the reaction of fluosilicic acid and ammonia water, and after the reaction, high-dispersibility white carbon black is obtained after solid-liquid separation and drying; the reaction is to gradually add ammonia water to fluosilicic acid, monitor the system pH during the reaction, and when the system pH reaches 6-8, add the imidazole dispersant, and then age.

2. The method for preparing highly dispersible white carbon black according to claim 1, It is characterized in that The imidazole dispersant is selected from one or more of 2-methylimidazole, 2-ethyl-4-methylimidazole and diphenylimidazole.

3. The method for preparing highly dispersible white carbon black according to claim 1, It is characterized in that The amount of the imidazole dispersant added is 0.5 wt.% to 40 wt.% of the theoretical designed silica product mass.

4. The method for preparing highly dispersible white carbon black according to claim 1, It is characterized in that The reaction temperature is 10-95°C.

5. The method for preparing highly dispersible white carbon black according to claim 1, It is characterized in that The aging time is 0.1 to 3 hours.

6. The method for preparing highly dispersible white carbon black according to claim 1, It is characterized in that The concentration of the fluorosilicic acid is 10-35%, and the concentration of the ammonia water is 1-20 mol / L.

7. The method for preparing highly dispersible white carbon black according to claim 6, It is characterized in that After the aging, continue to add ammonia water to react to the end point.

8. The method for preparing highly dispersible white carbon black according to claim 7, It is characterized in that The pH of the system is monitored during the continuous addition of ammonia water. When the pH of the system is 8.1-9, the reaction is completed.