A recycled aggregate-steel slag carbon-fixing permeable brick and its preparation method

By using recycled aggregate and steel slag carbon sequestration technology in permeable bricks, combined with internal curing agent and carbonization maintenance technology, the problems of poor permeability and high energy consumption of traditional permeable bricks are solved, and efficient and environmentally friendly permeable brick preparation is achieved, with significant results. economic and environmental value.

CN117069459BActive Publication Date: 2024-11-26HUAXIN CEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310902068.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-21
Publication Date
2024-11-26
Estimated Expiration
2043-07-21

AI Technical Summary

Technical Problem

In the early stage of the blank forming, the steel slag structure is dense, the water permeability is poor, and the hydration effect is poor. The traditional steel slag permeable brick process has high energy consumption and the failure to effectively utilize steel slag and recycled aggregates, resulting in waste of resources and environmental pollution. .

Method used

Recycled aggregate - steel slag carbon-permeable bricks are used. After mixing the recycled aggregate with part of the water, adding internal curing agent to modify it, then adding steel slag micro powder and recycled micro powder, finally adding steel slag aggregate and residual water, and after forming and carbonization Curing and preparing to form permeable bricks with excellent mechanical and permeability.

Benefits of technology

The preparation of permeable bricks without cement and natural aggregates has been achieved, which significantly improves the mechanical properties and permeability of permeable bricks, reduces carbon emissions, reduces natural resource consumption and environmental pollution, and increases the added value of solid waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004352088160000071
    Figure BDA0004352088160000071
  • Figure BDA0004352088160000081
    Figure BDA0004352088160000081
Patent Text Reader

Abstract

The invention discloses a recycled aggregate-steel slag carbon-fixing permeable brick and a preparation method thereof. The raw materials of the permeable brick include a cementitious material, an aggregate, water and an internal curing agent; wherein: the cementitious material is steel slag micropowder and recycled micropowder, and the recycled micropowder accounts for 10-30% of the cementitious material; the aggregate is steel slag aggregate and recycled aggregate, and the recycled aggregate accounts for 30-70wt% of the aggregate; the internal curing agent accounts for 1.2-3.5% of the cementitious material; the water-cement ratio is 0.27-0.33, and the bone-cement ratio is 3.0-4.0; the permeable brick is modified by adding an internal curing agent after mixing the recycled aggregate with part of the water; then adding steel slag micropowder and recycled micropowder to wrap the recycled aggregate, and finally adding steel slag aggregate and the remaining water, and then carbonizing after molding and curing. The permeable brick has good mechanical properties and water permeability, and has a significant carbon-fixing effect. It can make full use of solid waste resources, improve the added value of solid waste, and has important economic and environmental value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of permeable bricks, and in particular relates to a recycled aggregate-steel slag carbon-fixing permeable brick and a preparation method thereof. Background Art

[0002] In 2022, my country's total crude steel output will be 840 million tons, and the total output of all steel slag will be 137 million tons. At present, the comprehensive utilization of steel slag is mainly iron selection, with a comprehensive utilization of about 18 million tons, followed by the utilization of steel slag as building materials, with a usage of about 16 million tons, accounting for about 11.68% of the total amount of steel slag produced, and other utilizations of about 3 million tons, with a total utilization of 37 million tons. It can be seen that only about 27% of steel slag is effectively utilized. A large amount of piled steel slag not only seriously occupies limited land resources, but also causes many environmental problems, causing soil, surface water and groundwater pollution. At the same time, the construction industry consumes a large amount of natural sand and stone every year. Sand and stone are non-renewable resources in the short term. Faced with a large amount of mountain quarrying, it will inevitably lead to the deterioration of the ecological environment and the emergence of a resource crisis. At the same time, the amount of waste concrete generated by construction and demolition is huge every year. If it is not utilized, it will cause a waste of resources and increase environmental pressure. Making construction waste into recycled aggregates for utilization can greatly alleviate this situation.

[0003] The construction of "sponge city" is inseparable from the permeable materials of the road surface. Permeable bricks are a kind of porous products. The permeable brick pavement can effectively absorb the infiltration of rainwater, replenish groundwater resources, improve the thermal environment of urban life, absorb urban noise, and improve the ecological environment of urban surface soil. At present, the cementitious material of permeable bricks mostly adopts traditional silicate cement, but there is a problem of excessive energy consumption. Steel slag aggregate and recycled aggregate are also used in permeable bricks to replace natural aggregates. However, at present, the traditional steel slag permeable bricks are relatively dense in the early stage of the blank forming, and the pores of the permeable bricks are large, so the internal water is easy to evaporate, thereby weakening the hydration effect of the steel slag and reducing the hydration product calcium hydroxide, which is not conducive to the initial strength growth of the blank. If the additional water is supplemented, not only the process is cumbersome, but also manpower and material resources are wasted. When the water content is not well controlled, it will also be detrimental to the initial strength of the blank.

[0004] Therefore, how to apply steel slag and recycled aggregates to permeable bricks and achieve excellent performance without using cement and natural aggregates is of great economic and environmental significance. Summary of the invention

[0005] The purpose of the present invention is to provide a recycled aggregate-steel slag carbon fixation permeable brick and a preparation method thereof. The permeable brick has good mechanical properties and water permeability, and at the same time, the permeable brick has a significant carbon fixation effect, which is conducive to reducing carbon emissions, does not require the use of cement and natural aggregates, makes full use of solid waste resources, reduces excessive consumption of natural resources, reduces solid waste pollution to the environment, and increases the added value of solid waste, and has important economic value and environmental value.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] Provided is a recycled aggregate-steel slag carbon-fixing permeable brick, the raw materials of which include cementitious material, aggregate, water and internal curing agent; wherein:

[0008] The cementitious materials are steel slag powder and recycled powder. By mass percentage, the recycled powder accounts for 10-30% of the cementitious materials; the internal curing agent accounts for 1.2-3.5% of the cementitious materials;

[0009] The aggregates are steel slag aggregates and recycled aggregates, and the recycled aggregates account for 30-70% of the aggregates by mass percentage;

[0010] The water-cement ratio is 0.27-0.33, and the bone-cement ratio is 3.0-4.0;

[0011] The permeable brick is prepared by mixing recycled aggregate with part of water and then adding internal curing agent for modification; then adding steel slag powder and recycled powder to wrap the recycled aggregate, and finally adding steel slag aggregate and remaining water, and then performing molding curing and carbonization curing.

[0012] According to the above scheme, the particle size of the recycled aggregate is 5-16 mm, the water absorption rate of the recycled aggregate is ≤3%, and the crushing value is ≤20%.

[0013] According to the above scheme, the particle size of the steel slag aggregate is 2-10 mm, and the crushing value is ≤12%.

[0014] According to the above scheme, the specific surface area of ​​the steel slag powder is 500-600m 2 / kg, CaO content 35-45%.

[0015] According to the above scheme, the specific surface area of ​​the regenerated micro powder is 400-500m 2 / kg, CaO content 10-25%.

[0016] According to the above scheme, the internal curing agent is at least one of anhydrous calcium sulfate whiskers, sodium alginate, and sodium polyacrylate.

[0017] Preferably, when the internal curing agent is a mixture of anhydrous calcium sulfate whiskers, sodium alginate and sodium polyacrylate, by mass percentage, the anhydrous calcium sulfate whiskers are added in an amount of 1-3% of the amount of the cementitious material, the sodium alginate is added in an amount of 0.1-0.3% of the amount of the cementitious material, and the sodium polyacrylate is added in an amount of 0.1-0.2% of the amount of the cementitious material.

[0018] According to the above scheme, the recycled aggregate is mixed with water accounting for 40-70% of the total water content and then an internal curing agent is added for modification.

[0019] According to the above scheme, the carbonization curing temperature after demoulding is 50-90°C, the CO2 concentration is 20%-99.9%, the carbonization pressure is 0.1-1.0MPa, the relative humidity is not less than 65%, and the time is 2-24 hours.

[0020] A method for preparing the above-mentioned recycled aggregate-steel slag carbon-fixing permeable brick is provided, comprising the following steps:

[0021] 1) Mix the recycled aggregate and part of the water evenly, then add the internal curing agent to moisten the surface of the recycled aggregate to a saturated surface dry state;

[0022] 2) Continue to add steel slag powder and recycled powder and stir evenly to form a cementitious material slurry shell to wrap the surface of the aggregate;

[0023] 3) Finally, add steel slag aggregate and remaining water, stir evenly, perform molding and curing, and then perform carbonization and curing to obtain the recycled aggregate-steel slag carbon-fixed permeable brick.

[0024] According to the above scheme, in step 1), the recycled aggregate is mixed evenly with water accounting for 40-70% of the total water.

[0025] According to the above scheme, in step 2), the stirring time is 5-8 minutes.

[0026] According to the above scheme, in step 3), the stirring time is 3-5 minutes.

[0027] According to the above scheme, in step 3), the molding and curing time is 12-24 hours.

[0028] According to the above scheme, in step 3), the molding and curing are as follows: pouring the obtained slurry into a mold, forming it by mechanical static pressure, and curing it for 12-24 hours after demolding.

[0029] Preferably, the static pressure molding pressure is 5-8Mpa, and the holding time is 2-4min.

[0030] Preferably, the curing temperature after demoulding is 20-30° C., and the relative humidity is not less than 65%.

[0031] According to the above scheme, in step 3), the carbonization curing temperature is 50-90°C, the CO2 concentration is 20%-99.9%, the carbonization pressure is 0.1-1.0MPa, and the relative humidity is not less than 65%.

[0032] According to the above scheme, in step 3), the carbonization curing time is 2-24 hours, preferably 16-20 hours.

[0033] The present invention provides a recycled aggregate-steel slag carbon-fixing permeable brick, the working mechanism of which is as follows:

[0034] The present invention uses steel slag, steel slag powder, construction waste recycled aggregate, and recycled powder as main raw materials, and utilizes their carbonization characteristics to fix carbon dioxide in mineral form while obtaining permeable bricks with high strength, good volume stability, high water permeability, and excellent durability; wherein:

[0035] The silicates such as tricalcium silicate and dicalcium silicate, and minerals such as free calcium oxide in steel slag not only have certain hydration and gelling activity, but also the hydration products such as calcium hydroxide have the carbonization characteristics of reacting with CO2 to form stable carbonates. The incompletely hydrated cement particles and hydration products calcium hydroxide and gel contained in the recycled aggregate and recycled micropowder also have carbonization characteristics. The finer carbonization products calcium carbonate and gel generated during carbonization fill the internal pores of the aggregate and make the aggregate interface bond more firmly, thereby improving the aggregate strength and interface strength, and the mechanical properties of the permeable bricks are improved in macroscopic performance. Due to the relatively dense structure of steel slag, the hydration rate of minerals such as tricalcium silicate, dicalcium silicate and free calcium oxide is slow. If ordinary standard maintenance is used, the strength of the permeable brick body will increase slowly due to the poor hydration activity and slow hydration rate of steel slag powder and recycled micropowder, resulting in a long production cycle of permeable bricks, which is not conducive to industrial mass production. At the same time, the permeable bricks produced have poor performance. The carbonization curing adopted in the present invention can improve the growth process of its physical properties and shorten the production cycle, and can also adsorb and solidify CO2.

[0036] Recycled aggregate and recycled micro powder have porous structure and carbonizable characteristics. After mixing recycled aggregate with some water in advance, internal curing agent is added for modification. On the one hand, internal curing agent can repair the cracks between recycled aggregate particles to a certain extent, making the bonding between aggregate particles of permeable bricks tighter, which will better promote the improvement of permeable brick performance. On the other hand, internal curing agent can modify the surface of recycled aggregate, improve its water absorption performance, and make it easier to release the absorbed water inside, which will better play the role of internal curing of recycled aggregate; at the same time, the adsorbed water in recycled aggregate can provide the required water for hydration of steel slag, play the role of internal curing, and provide certain water for the hydration of minerals such as tricalcium silicate, dicalcium silicate and free calcium oxide in steel slag, so that steel slag can be better hydrated to generate more calcium hydroxide. Calcium hydroxide is the main substance for carbonization reaction, so the use of internal curing method can promote the carbonization effect of permeable brick body.

[0037] The present invention has the following beneficial effects:

[0038] 1. The present invention provides a recycled aggregate-steel slag carbon-fixing permeable brick, which has good mechanical properties and permeability. At the same time, the permeable brick has a significant carbon-fixing effect, which is beneficial to reducing carbon emissions. The permeable brick of the present invention completely utilizes steel metallurgical solid waste steel slag, steel slag micropowder and construction waste recycled aggregate and recycled micropowder as raw materials, avoiding the use of traditional silicate cement and natural aggregate. It can not only reduce the pollution of solid waste to the environment and increase the added value of solid waste, but also reduce energy consumption and reduce the excessive consumption of natural resources. It has important economic value and environmental value.

[0039] 2. The present invention provides a method for preparing recycled aggregate-steel slag carbon-fixed permeable bricks. First, the recycled aggregate is mixed with part of water in advance and then an internal curing agent is added for modification to achieve the internal curing characteristics of the recycled aggregate. The early strength of the permeable brick body is improved by utilizing the recycled aggregate to internally cure steel slag aggregate and steel slag micropowder, and it is beneficial to promote the carbonization effect of the carbon water brick body. The recycled aggregate, recycled micropowder, steel slag aggregate, and steel slag micropowder have carbonizable characteristics, and the performance of the permeable brick is enhanced through carbonization reaction. The prepared recycled aggregate-steel slag carbon-fixed permeable brick has high strength, good volume stability, high permeability, and excellent durability.

[0040] 3. Utilizing the carbonizable properties of steel slag, steel slag powder, recycled aggregate and recycled powder, the carbonization process can not only improve the performance of permeable bricks, but also solidify and seal CO2, which is conducive to the realization of dual carbon goals. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. The test reagents used in the following embodiments, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0042] Example 1

[0043] A method for preparing the above-mentioned recycled aggregate-steel slag carbon-fixing permeable brick is provided, comprising the following steps:

[0044] The particle size of the recycled aggregate is 5-16mm, the particle size of the steel slag aggregate is 2-10mm, the total aggregate is 2.5kg, and the proportion of the recycled aggregate is 30%. The recycled aggregate is mixed with 100g of water, and then 1% of anhydrous calcium sulfate whisker, 0.1% of sodium alginate, and 0.1% of sodium polyacrylate are added as internal curing agents to make the surface of the recycled aggregate evenly wet. Then add 450g of steel slag powder and 175g of recycled powder, stir for 6 minutes to form a cementitious material slurry shell to wrap the surface of the aggregate, finally add steel slag aggregate and 68g of water, stir for 3 minutes and pour into the mold, use 8MPa mechanical static pressure to form, maintain the pressure for 3 minutes and then demold, cure for 20 hours at 20-30℃ and relative humidity of 65%, and then carbonize and cure in a carbonization kettle for 20 hours. The carbonization curing conditions are: carbonization temperature of 50℃, humidity of not less than 65%, pressure of 0.3MPa, and CO2 concentration of 99.9%, so as to obtain the recycled aggregate-steel slag solid carbon permeable brick.

[0045] In this embodiment, the specific surface area of ​​the steel slag powder is 550m 2 / kg, CaO content 40%; the specific surface area of ​​the regenerated micro powder is 450m 2 / kg, CaO content is 15%, recycled micro powder accounts for 28% in the rubber material; recycled aggregate water absorption rate ≤2.5%, crushing value ≤18%; steel slag aggregate crushing value ≤10%.

[0046] Example 2

[0047] A method for preparing the above-mentioned recycled aggregate-steel slag carbon-fixing permeable brick is provided, comprising the following steps:

[0048] The particle size of the recycled aggregate is 5-16mm, the particle size of the steel slag aggregate is 2-10mm, the total aggregate is 2.5kg, and the proportion of the recycled aggregate is 50%. The recycled aggregate is mixed with 100g of water evenly, and then 2% anhydrous calcium sulfate whisker, 0.2% sodium alginate, and 0.1% sodium polyacrylate are added as internal curing agents to make the surface of the recycled aggregate evenly wet. Then add 562.5g of steel slag powder and 62.5g of recycled powder, stir for 6 minutes to form a cementitious material slurry shell to wrap the surface of the aggregate, finally add steel slag aggregate and 87g of water, stir for 3 minutes and pour into the mold, use 8MPa mechanical static pressure to form, maintain the pressure for 3 minutes and then demold, cure for 24 hours at 20-30℃ and relative humidity of 65%, and then carbonize and cure for 20 hours in a carbonization kettle, with a carbonization temperature of 50℃, a humidity of not less than 65%, a pressure of 0.6MPa, and a CO2 concentration of 99.9%, to obtain the recycled aggregate-steel slag solid carbon permeable brick.

[0049] In this embodiment, the specific surface area of ​​the steel slag powder is 500m 2 / kg, CaO content 40%; the specific surface area of ​​the regenerated micro powder is 400m 2 / kg, CaO content 10%, recycled micro powder accounts for 10% of the rubber material. The water absorption rate of recycled aggregate is ≤2.5%, the crushing value is ≤18%; the crushing value of steel slag aggregate is ≤10%.

[0050] Example 3

[0051] A method for preparing the above-mentioned recycled aggregate-steel slag carbon-fixing permeable brick is provided, comprising the following steps:

[0052] The particle size of the recycled aggregate is 5-16mm, the particle size of the steel slag aggregate is 2-10mm, the total aggregate is 2.5kg, and the proportion of the recycled aggregate is 70%. The recycled aggregate is mixed with 100g of water evenly, and then 3% anhydrous calcium sulfate whisker, 0.3% sodium alginate, and 0.2% sodium polyacrylate are added as internal curing agents to make the surface of the recycled aggregate evenly wet. Then add 562.5g of steel slag powder and 62.5g of recycled powder, stir for 6 minutes to form a cementitious material slurry shell to wrap the surface of the aggregate, finally add steel slag aggregate and 106g of water, stir for 3 minutes and pour into the mold, use 8MPa mechanical static pressure to form, maintain the pressure for 3 minutes and then demold, cure at 20-30℃, relative humidity 65% ​​for 24 hours, and then carbonize and cure in a carbonization kettle for 20 hours, the carbonization temperature is 50℃, the humidity is not less than 65%, the pressure is 0.6MPa, and the CO2 concentration is 20%, so as to obtain the recycled aggregate-steel slag solid carbon permeable brick.

[0053] In this embodiment, the specific surface area of ​​the steel slag powder is 550m 2 / kg, CaO content 35%, regenerated micro powder specific surface area 400m2 / kg, CaO content 10%, recycled micro powder accounts for 10% of the rubber material. The water absorption rate of recycled aggregate is ≤2.5%, and the crushing value is ≤18%. The crushing value of steel slag aggregate is ≤10%.

[0054] Example 4

[0055] A method for preparing the above-mentioned recycled aggregate-steel slag carbon-fixing permeable brick is provided, comprising the following steps:

[0056] The particle size of the recycled aggregate is 5-16mm, the particle size of the steel slag aggregate is 2-10mm, the total aggregate is 2.5kg, and the proportion of the recycled aggregate is 70%. The recycled aggregate is mixed with 100g of water evenly, and then 3% anhydrous calcium sulfate whisker, 0.3% sodium alginate, and 0.2% sodium polyacrylate are added as internal curing agents to make the surface of the recycled aggregate evenly wet. Then add 562.5g of steel slag powder and 62.5g of recycled powder, stir for 6 minutes to form a cementitious material slurry shell to wrap the surface of the aggregate, finally add steel slag aggregate and 106g of water, stir for 3 minutes and pour into the mold, use 8MPa mechanical static pressure to form, maintain the pressure for 3 minutes and then demold, cure at 20-30℃, relative humidity 65% ​​for 24 hours, and then carbonize and cure in a carbonization kettle for 2 hours, the carbonization temperature is 70℃, the humidity is not less than 65%, the pressure is 0.3MPa, and the CO2 concentration is 20%, so as to obtain the recycled aggregate-steel slag solid carbon permeable brick.

[0057] In this embodiment, the specific surface area of ​​the steel slag powder is 550m 2 / kg, CaO content 35%, regenerated micro powder specific surface area 400m 2 / kg, CaO content 10%, recycled micro powder accounts for 10% of the rubber material. The water absorption rate of recycled aggregate is ≤2.5%, the crushing value is ≤18%; the crushing value of steel slag aggregate is ≤10%.

[0058] Comparative Example 1

[0059] The proportion and molding method of the recycled aggregate-steel slag permeable bricks in this comparative example are the same as those in Example 1, but the carbonization curing method is not adopted.

[0060] The particle size of the recycled aggregate is 5-16mm, the particle size of the steel slag aggregate is 2-10mm, the aggregate is 2.5kg in total, and the proportion of the recycled aggregate is 30%. The recycled aggregate is mixed with 100g of water evenly, and then 1% of anhydrous calcium sulfate whisker, 0.1% of sodium alginate, and 0.1% of sodium polyacrylate are added as internal curing agents to make the surface of the recycled aggregate reach a uniform wetting state. Then 450g of steel slag powder and 175g of recycled powder are added, and stirred for 6min to form a cementitious material slurry shell to wrap the surface of the aggregate. Finally, steel slag aggregate and 68g of water are added, stirred for 3min, and then poured into the mold, and 8MPa mechanical static pressure is used for molding. After maintaining the pressure for 3min, demoulding is carried out, and curing is carried out for 20h at 20-30℃ and relative humidity of 65%.

[0061] In this comparative example, the specific surface area of ​​the steel slag powder is 550m 2 / kg, CaO content 40%, regenerated micro powder specific surface area 450m 2 / kg, CaO content 15%, recycled micro powder accounts for 28% of the rubber material. The water absorption rate of recycled aggregate is ≤2.5%, the crushing value is ≤18%; the crushing value of steel slag aggregate is ≤10%.

[0062] Comparative Example 2

[0063] The proportion and molding method of the recycled aggregate-steel slag permeable bricks in this comparative example are the same as those in Example 1, but the conventional standard curing method is adopted for curing for 28 days.

[0064] The particle size of the recycled aggregate is 5-16mm, the particle size of the steel slag aggregate is 2-10mm, the aggregate is 2.5kg in total, and the proportion of the recycled aggregate is 30%. The recycled aggregate is mixed with 100g of water evenly, and then 1% of anhydrous calcium sulfate whisker, 0.1% of sodium alginate, and 0.1% of sodium polyacrylate are added as internal curing agents to make the surface of the recycled aggregate reach a uniform wetting state. Then 450g of steel slag powder and 175g of recycled powder are added, and stirred for 6min to form a cementitious material slurry shell to wrap the surface of the aggregate. Finally, the steel slag aggregate and 68g of water are added, stirred for 3min, and then poured into the mold, and 8MPa mechanical static pressure is used for molding. After holding the pressure for 3min, demoulding is carried out, and curing is carried out under standard curing conditions for 28d.

[0065] In this comparative example, the specific surface area of ​​the steel slag powder is 550m 2 / kg, CaO content 40%, regenerated micro powder specific surface area 450m 2 / kg, CaO content 15%, recycled micro powder accounts for 28% of the rubber material. The water absorption rate of recycled aggregate is ≤2.5%, the crushing value is ≤18%; the crushing value of steel slag aggregate is ≤10%.

[0066] Comparative Example 3

[0067] The proportion and molding method of the recycled aggregate-steel slag permeable brick in this comparative example are the same as those in Example 2, but recycled aggregate and internal curing agent are not used.

[0068] The steel slag aggregate particle size is selected to be 2-10mm, and the aggregate is 2.5kg in total. 30% of the steel slag aggregate is mixed with 100g of water to make the surface of the steel slag aggregate evenly wetted. Then 562.5g of steel slag powder and 62.5g of recycled powder are added, and stirred for 6 minutes to form a cementitious material slurry shell to wrap the aggregate surface. Finally, the remaining steel slag aggregate and 87g of water are added, stirred for 3 minutes, and poured into the mold. The mold is formed by 8MPa mechanical static pressure, and the mold is demolded after holding the pressure for 3 minutes. After curing for 24 hours at 20-30℃ and relative humidity of 65%, it is carbonized and cured in a carbonization kettle for 20 hours. The carbonization temperature is 50℃, the humidity is not less than 65%, the pressure is 0.6MPa, and the CO2 concentration is 99.9%. The permeable brick can be obtained.

[0069] In this comparative example, the specific surface area of ​​the steel slag powder is 500m 2 / kg, CaO content 40%, regenerated micro powder specific surface area 400m 2 / kg, CaO content 10%, recycled micro powder accounts for 10% in the rubber material. The crushing value of steel slag aggregate is ≤10%.

[0070] Comparative Example 4

[0071] The proportion and molding method of the recycled aggregate-steel slag permeable bricks in this comparative example are the same as those in Example 3, but steel slag aggregate is not used.

[0072] The particle size of the recycled aggregate is 5-9.5mm, and the total amount of aggregate is 2.5kg. 30% of the recycled aggregate is mixed with 100g of water, and then 3% of anhydrous calcium sulfate whisker, 0.3% of sodium alginate, and 0.2% of sodium polyacrylate are added as internal curing agents to make the surface of the recycled aggregate reach a uniform wet state. Then 562.5g of steel slag powder and 62.5g of recycled powder are added, and stirred for 6min to form a cementitious material slurry shell to wrap the surface of the aggregate. Finally, the remaining recycled aggregate and 106g of water are added, stirred for 3min, and then poured into the mold, and 8MPa mechanical static pressure is used for molding. After holding the pressure for 3min, demolding is carried out, and curing is carried out for 24h at 20-30℃ and relative humidity of 65%, and then carbonization curing is carried out in a carbonization kettle for 20h. The carbonization temperature is 50℃, the humidity is not less than 65%, the pressure is 0.6MPa, and the CO2 concentration is 20%, and the permeable brick can be obtained.

[0073] In this comparative example, the specific surface area of ​​the steel slag powder is 550m 2 / kg, CaO content 35%, regenerated micro powder specific surface area 400m 2 / kg, CaO content 10%, recycled micro powder accounts for 10% of the rubber material. The water absorption rate of recycled aggregate is ≤2.5%, and the crushing value is ≤18%.

[0074] The mechanical properties, water permeability and carbon fixation effects of the permeable bricks corresponding to Examples 1, 2, 3, 4 and Comparative Examples 1, 2, 3, 4 are shown in Table 1.

[0075] Table 1. Performance test of recycled aggregate-slag permeable bricks with different proportions or systems

[0076]

[0077]

[0078] It can be seen from Table 1 that the recycled aggregate internal curing and coordinated carbonization curing system obtained in the embodiment of the present invention can significantly improve the mechanical properties of the recycled aggregate-steel slag permeable brick, while having good permeability, and the permeable brick has a significant carbon fixation effect, which can achieve the goal of reducing carbon emissions.

[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution, improvement, etc. made by any technician familiar with the technical scope disclosed in the present invention shall be included in the protection scope of the present invention.

Claims

1. A recycled aggregate-steel slag carbon-fixing permeable brick, characterized in that: The raw materials of permeable bricks include cementitious materials, aggregates, water and internal curing agents; among which: The cementitious materials are steel slag powder and recycled powder. By mass percentage, the recycled powder accounts for 10-30% of the cementitious materials; the internal curing agent accounts for 1.2-3.5% of the cementitious materials; Aggregates are steel slag aggregates and recycled aggregates, with recycled aggregates accounting for 30-70% of the aggregates by mass; The water-cement ratio is 0.27-0.33, and the bone-cement ratio is 3.0-4.0; The permeable brick is prepared by mixing recycled aggregate with part of water and then adding internal curing agent for modification; then adding steel slag powder and recycled powder to wrap the recycled aggregate, and finally adding steel slag aggregate and remaining water, and then performing molding curing and carbonization curing.

2. The permeable brick according to claim 1, characterized in that: The internal curing agent is at least one of anhydrous calcium sulfate whiskers, sodium alginate, and sodium polyacrylate.

3. The permeable brick according to claim 2, characterized in that: When the internal curing agent is a mixture of anhydrous calcium sulfate whiskers, sodium alginate and sodium polyacrylate, calculated by mass percentage, the amount of anhydrous calcium sulfate whiskers is 1%-3% of the amount of cementitious material, the amount of sodium alginate is 0.1%-0.3% of the amount of cementitious material, and the amount of sodium polyacrylate is 0.1%-0.2% of the amount of cementitious material.

4. The permeable brick according to claim 1, characterized in that: The carbonization curing temperature is 50-90° C., the CO2 concentration is 20%-99.9%, the carbonization pressure is 0.1-1.0 MPa, the relative humidity is not less than 65%, and the time is 2-24 hours.

5. The permeable brick according to claim 1, characterized in that: The particle size of the recycled aggregate is 5-16 mm, the water absorption rate of the recycled aggregate is ≤3%, and the crushing value is ≤20%; the particle size of the steel slag aggregate is 2-10 mm, and the crushing value is ≤12%.

6. The permeable brick according to claim 1, characterized in that: The specific surface area of ​​the steel slag powder is 500-600m 2 / kg, CaO content 35-45%; the specific surface area of ​​the regenerated micro powder is 400-500 m 2 / kg, CaO content 10-25%.

7. A method for preparing the recycled aggregate-steel slag carbon-fixing permeable brick according to any one of claims 1 to 6, characterized in that: The following steps are involved: 1) Mix the recycled aggregate with part of the water evenly, then add the internal curing agent to moisten the surface of the recycled aggregate to a saturated surface dry state; 2) Continue to add steel slag powder and recycled powder and stir evenly to form a cementitious material slurry shell to wrap the surface of the aggregate; 3) Finally, add steel slag aggregate and remaining water, stir evenly, and then perform molding and curing, and then perform carbonization and curing to obtain recycled aggregate-steel slag solid carbon permeable bricks.

8. The preparation method according to claim 7, characterized in that: In the step 2), the stirring time is 5-8 minutes; in the step 3), the stirring time is 3-5 minutes.

9. The preparation method according to claim 7, characterized in that: In the step 3), the molding and curing time is 12-24 hours.

10. The preparation method according to claim 7, characterized in that: In the step 3), the carbonization curing temperature is 50-90°C, the CO2 concentration is 20%-99.9%, the carbonization pressure is 0.1-1.0MPa, the relative humidity is not less than 65%, and the time is 2-24h.