A method for determining zirconium oxide content in dispersion-strengthened platinum-based materials

The total zirconium and solid-solution zirconium content was measured by inductively coupled plasma atomic emission spectrometer, and the zirconium oxide content was calculated indirectly, which solved the problem of inaccurate determination of zirconium oxide content in the prior art, achieved more accurate and rapid measurement results, and reduced the Sample loss.

CN117092090BActive Publication Date: 2024-12-06CHONGQING MATERIALS RES INST

Patent Information

Application Number
CN202310855312.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-12
Publication Date
2024-12-06
Estimated Expiration
2043-07-12

AI Technical Summary

Technical Problem

The determination of the zirconium oxide content in diffusion-strengthening platinum-based materials in the prior art is not accurate enough, resulting in insufficient guidance on production processes and product performance.

Method used

The total zirconium and solid-solution zirconium content was measured by inductively coupled plasma atomic emission spectrometer, and the zirconium oxide content was measured indirectly through the differences in dissolution properties of Zr and ZrO2, and the test solution was prepared using hydrochloric acid and nitric acid mixed acid to reduce sample loss and improve measurement accuracy. .

Benefits of technology

The accurate determination of the zirconium oxide content in the diffusely enhanced platinum-based material is achieved. The method is simple and fast, the sample loss is low, and the detection results are more accurate and reliable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117092090B_ABST
    Figure CN117092090B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for determining the content of zirconium oxide in a dispersion-strengthened platinum-based material. The method uses a mixed acid dissolution of hydrochloric acid and nitric acid to prepare a solid-solution zirconium test solution for reacting and dissolving zirconium in a material by using the difference in the solubility properties of zirconium and zirconium oxide; and uses a mixed acid dissolution of hydrochloric acid and nitric acid plus hydrofluoric acid to prepare a total zirconium test solution for dissolving zirconium and zirconium oxide contained in the material, that is, total zirconium. On an inductively coupled plasma atomic emission spectrometer, the emission spectrum intensity of the zirconium element in the test solution is measured at a recommended wavelength, the mass fractions of total zirconium and solid-solution zirconium are calculated from a calibration curve, and the content of zirconium oxide in the dispersion-strengthened platinum-based material is calculated by subtracting the mass fraction of solid-solution zirconium from the mass fraction of total zirconium. The method of the present invention has low sample loss, is simple and fast, and has more accurate and reliable results.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for determining a substance in a material, and in particular to a method for determining the content of zirconium oxide in a dispersion-strengthened platinum-based material. Background Art

[0002] Dispersion-strengthened platinum materials have higher high-temperature strength, creep resistance and corrosion resistance than unstrengthened platinum, and are key materials for making crucibles and glass fiber bushings for the glass industry. How to introduce and add dispersion-strengthened particles to the base metal material is the key to preparing dispersion-strengthened platinum materials, and the introduction method or method has a great influence on the high-temperature performance of dispersion-strengthened platinum materials.

[0003] Among them, zirconium oxide dispersion strengthened platinum material uses trace zirconium oxide as a stable second phase, evenly distributed in the platinum matrix, which prevents grain boundary sliding and improves the strength and high-temperature creep resistance of platinum. The production and preparation of the material is mostly carried out with metal zirconium, which is then converted into zirconium oxide. Therefore, the oxidation efficiency of the strengthened metal zirconium determines the content of zirconium oxide in the material, production energy consumption, stability, etc.

[0004] At present, there are many studies on the preparation methods, microstructure and properties of zirconium oxide dispersion-strengthened platinum materials. Among them, the article by Xie Zineng et al. specifically studied the effects of different zirconium oxide contents on the room temperature physics, mechanics and high temperature sustained fracture life of dispersion-strengthened platinum. Xu Wenge also pointed out that when the zirconium oxide content is about 0.3%, the strength and processing properties of dispersion-strengthened platinum can be taken into account. Therefore, accurately determining the zirconium oxide content in zirconium oxide dispersion-strengthened platinum-based materials can guide the production process, clarify product performance and improve the yield rate.

[0005] However, the method for testing the zirconium oxide content in the material in the prior art is to use the difference in solubility properties of metal zirconium and zirconium oxide in the metal alloy material, weigh the zirconium oxide after precipitation and crystallization, and then calculate the content of zirconium oxide in the dispersion-strengthened platinum-based material to determine its strength and processing properties. However, the above method inevitably causes process losses during the weighing of zirconium oxide, resulting in inaccurate determination of the zirconium oxide content. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for determining the content of zirconium oxide in a dispersion-strengthened platinum-based material, which solves the problem of inaccurate measurement of the content of zirconium oxide in a dispersion-strengthened platinum-based material in the prior art.

[0007] To achieve the above object, the technical solution of the present invention is:

[0008] The method for determining the content of zirconium oxide in dispersion-strengthened platinum-based materials comprises the following steps:

[0009] 1) Take two samples of dispersion-strengthened platinum-based material, set the mass of sample 1 to m1 and the mass of sample 2 to m2, and keep them for later use;

[0010] 2) Preparation of test solution:

[0011] Prepare a total zirconium test solution and a total zirconium sample blank test solution; a solid solution zirconium test solution and a solid solution zirconium sample blank test solution;

[0012] 3) Calibration curve drawing:

[0013] A standard solution with a zirconium content of 1000 μg / mL was selected to prepare a standard solution with a zirconium concentration of 100 μg / mL; 0.00 ml, 0.50 ml, 1.00 ml, 2.00 ml, 3.00 ml, 4.00 ml, 5.00 ml, and 10.00 ml of the zirconium standard solution were respectively added with a mixed acid of hydrochloric acid and nitric acid and hydrofluoric acid, wherein the volume ratio of the mixed acid to hydrofluoric acid was 10 to 5:1, and the solution was diluted to 100 ml with water, and shaken well to prepare a series of calibration solutions;

[0014] The intensity of the zirconium element in the above series of calibration solutions is tested at a wavelength of 343.8 nm or 339.1 nm in the spectrometer, and a calibration curve is drawn with the intensity of the zirconium element as the ordinate and the mass concentration as the abscissa;

[0015] 4) Calculation of zirconium element mass concentration in test solution:

[0016] The emission intensity of zirconium element in the total zirconium test solution, the total zirconium sample blank test solution, the solid solution zirconium test solution and the solid solution zirconium sample blank test solution is tested at a spectrometer wavelength of 343.8 nm or 339.1 nm, and the mass concentration of zirconium element in the total zirconium test solution, the total zirconium sample blank test solution, the solid solution zirconium test solution and the solid solution zirconium sample blank test solution is calculated using the following formula corresponding to the calibration curve drawn with the standard solution in step 3):

[0017]

[0018] Where:

[0019] ω—mass fraction of zirconium oxide, in %;

[0020] ρ1—mass concentration of zirconium in the total zirconium test solution of the sample, in μg / mL;

[0021] —Mass concentration of zirconium in the blank solution of the total zirconium sample, in μg / mL;

[0022] m1—the mass of the total zirconium sample tested, in g;

[0023] V1—total zirconium test solution volume of the sample, in mL;

[0024] ρ2—mass concentration of zirconium element in the sample solid solution zirconium test solution, in μg / mL;

[0025] —Mass concentration of zirconium element in blank solution of solid solution zirconium sample, in μg / mL;

[0026] m2—the mass of the solid solution zirconium sample tested, in g;

[0027] V2—volume of sample solid solution zirconium test solution, in mL;

[0028] 1.3509—Coefficient for converting zirconium to zirconium oxide.

[0029] Step 1) The particle size of the sample is less than 0.5 mm

[0030] The specific steps of preparing the test solution in step 2) are as follows:

[0031] 2.1) Preparation of total zirconium test solution

[0032] Add a mixture of hydrochloric acid and nitric acid and hydrofluoric acid to sample 1, heat to dissolve, cool to room temperature, and adjust the volume to 100 ml, record the volume as V1, and set aside;

[0033] 2.2) Preparation of blank test solution for total zirconium sample

[0034] Take a mixture of hydrochloric acid and nitric acid and hydrofluoric acid, heat and dissolve them, cool to room temperature, and dilute to 100 ml for later use;

[0035] 2.3) Preparation of solid solution zirconium test solution

[0036] Add a mixture of hydrochloric acid and nitric acid to sample 2, heat to dissolve, cool to room temperature, filter and precipitate, and then adjust the volume to 100 ml, record the volume as V2, and set aside;

[0037] 2.4) Preparation of blank test solution for solid solution zirconium sample

[0038] Take a mixture of hydrochloric acid and nitric acid, heat to dissolve, cool to room temperature, make up to 100 ml, and set aside.

[0039] The density of the nitric acid is 1.42 g / mL, the density of the hydrochloric acid is 1.19 g / mL, and the density of the hydrofluoric acid is 1.18 g / mL.

[0040] The spectrometer is an inductively coupled plasma atomic emission spectrometer.

[0041] The volume ratio of hydrochloric acid to nitric acid in the mixed acid is 3:1.

[0042] The volume ratio of the mixed acid to the hydrofluoric acid is 10:1.

[0043] In step 2.3), the precipitate is zirconium oxide.

[0044] The heating and dissolving in step 2.3) and step 2.4) are performed by electric heating when the material to be tested is a platinum-based alloy; and by microwave digestion when the material to be tested is a platinum-rhodium alloy.

[0045] The microwave digestion instrument has programmable temperature, pressure and time control, can monitor pressure and temperature during the digestion process, and is used in conjunction with a clamping device, a protective device and a pressure relief device.

[0046] The method of the present invention uses the difference in solubility properties of Zr and ZrO2 to measure the total Zr and solid solution Zr contents using an inductively coupled plasma atomic emission spectrometer, and indirectly measures the ZrO2 content. The measurement result is accurate, the method is simple and fast, and the sample loss is small.

[0047] Beneficial effects of the present invention:

[0048] 1. The present invention uses a mixed acid of hydrochloric acid and nitric acid to dissolve the zirconium in the material to prepare a solid solution zirconium test solution, which is used to react and dissolve the zirconium in the material; uses a mixture of hydrochloric acid and nitric acid plus hydrofluoric acid to dissolve the zirconium and zirconium oxide in the material to prepare a total zirconium test solution, which is used to dissolve the zirconium and zirconium oxide contained in the material, that is, the total zirconium. On an inductively coupled plasma atomic emission spectrometer, the emission spectrum intensity of the zirconium element in the test solution is measured at the recommended wavelength, and the mass fraction of the zirconium element in the total zirconium + solid solution zirconium is calculated from the calibration curve. The content of zirconium oxide in the dispersion-strengthened platinum-based material is calculated by subtracting the mass fraction of the solid solution zirconium from the mass fraction of the total zirconium. The zirconium oxide content in the dispersion-strengthened platinum-based material detected by the method of the present invention is an indirect measurement. The method is simple and fast, with less sample loss, and the test results are more accurate and reliable.

[0049] 2. In the determination method of the present invention, a blank test solution is prepared at the same time as the total zirconium test solution and the solid solution zirconium test solution. When the total zirconium and solid solution zirconium zirconium element contents of the sample are detected, the zirconium element content of the blank test solution is subtracted, so that the measurement of the total zirconium and solid solution zirconium in the sample is more accurate, and thus the measurement of the zirconium oxide content in the dispersion-strengthened platinum-based material is more accurate.

[0050] The present invention uses the difference in solubility performance between Zr and ZrO2 to determine the total Zr and solid solution Zr contents using an inductively coupled plasma atomic emission spectrometer, and indirectly determines the ZrO2 content. The determination result is accurate, the method is simple and fast, and the sample loss is small. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 is the calibration curve of zirconium mass concentration;

[0052] Figure 2 is the calibration curve of zirconium mass concentration. DETAILED DESCRIPTION

[0053] All reagents in this example are commercial reagents.

[0054] Example 1 Measurement of zirconium oxide content in platinum-rhodium alloy material

[0055] S1. Take samples. Take two samples of particles with a particle size of less than 0.5 mm. Accurately weigh 0.05 g of each sample to an accuracy of 0.0001. Mark the mass of sample 1 as m1 and the mass of sample 2 as m2 for later use.

[0056] S2. Preparation of test solution

[0057] Prepare total zirconium test solution, total zirconium sample blank test solution, solid solution zirconium test solution and solid solution zirconium sample blank test solution. The volume of the total zirconium test solution is marked as V1, and the volume of the solid solution zirconium test solution is marked as V2.

[0058] S21. Preparation of total zirconium test solution

[0059] Place sample 1 in a 100mL polytetrafluoroethylene microwave digestion tank, add 20mL of a mixture of hydrochloric acid and nitric acid and 2mL of hydrofluoric acid, place in a microwave digestion instrument and heat to dissolve. After the end, cool, transfer to a 100mL plastic volumetric flask and dilute to 100mL, record the volume as V1, and set aside;

[0060] S22. Preparation of blank test solution for total zirconium sample

[0061] Add 20 mL of a mixture of hydrochloric acid and nitric acid and 2 mL of hydrofluoric acid to a 100 mL polytetrafluoroethylene microwave digestion tank, place in a microwave digestion apparatus and heat to dissolve. After the end, cool, transfer to a 100 mL plastic volumetric flask and dilute to 100 mL for later use;

[0062] S23. Preparation of solid solution zirconium test solution

[0063] Place sample 2 in a 100mL polytetrafluoroethylene microwave digestion tank, add 20mL of a mixture of hydrochloric acid and nitric acid, heat to dissolve, cool, transfer to a 100mL volumetric flask and dilute to 100mL, the volume is recorded as V2, and set aside; after heating to dissolve the metal sample, white powdery zirconium oxide will be present at the bottom of the container when cooling, filter the zirconium oxide powder to prevent it from being adsorbed into the equipment during the test and damaging the service life of the equipment.

[0064] This embodiment is to detect the content of zirconium oxide in the dispersion-strengthened platinum-rhodium alloy, and therefore, a microwave digestion apparatus is used for heating and dissolution.

[0065] S24. Preparation of blank test solution for solid solution zirconium sample

[0066] Add 20 mL of a mixture of hydrochloric acid and nitric acid into a 100 mL polytetrafluoroethylene microwave digestion vessel, transfer to a 100 mL plastic volumetric flask and dilute to 100 mL for later use;

[0067] S3. Calibration curve drawing

[0068] Select a standard solution with a zirconium content of 1000μg / mL, take 10.00mL and place it in a 100mL polytetrafluoroethylene volumetric flask, add 2mL hydrofluoric acid and 10mL nitric acid, add water to dilute the standard solution to 100μg / mL, respectively transfer 0.00ml, 0.50mL, 1.00mL, 2.00mL, 3.00mL, 4.00mL, 5.00mL, 10.00mL of the diluted solution into 8 100mL plastic volumetric flasks, add 10mL of a mixture of hydrochloric acid and nitric acid and 2mL of hydrofluoric acid, dilute with water, and shake well;

[0069] The density of the nitric acid is 1.42 g / mL, the density of the hydrochloric acid is 1.19 g / mL, the density of the hydrofluoric acid is 1.18 g / mL, and the mixed acid ratio of the hydrochloric acid and the nitric acid is 3:1.

[0070] The intensity of zirconium in the diluted standard solution was tested by inductively coupled plasma atomic emission spectrometer at a wavelength of 343.823 nm. The calibration curve was drawn with the emission spectrum intensity of zirconium as the ordinate and the mass concentration as the abscissa. Figure 1 , and establish a binary linear equation to obtain the relationship between the zirconium spectral intensity I and the zirconium mass concentration ρ:

[0071] I=aρ+b

[0072] Where:

[0073] I—light intensity of zirconium element;

[0074] ρ—mass concentration of zirconium element;

[0075] a — coefficient of the variable;

[0076] b—coefficient of the variable;

[0077]

[0078] It turns out that I = 7426.8ρ-130.25

[0079] S4. Calculate the mass concentration of zirconium in the test solution. Use an inductively coupled plasma atomic emission spectrometer to detect the emission intensity of zirconium in the total zirconium test solution, the total zirconium sample blank test solution, the solid solution zirconium test solution and the solid solution zirconium sample blank test solution at a wavelength of 343.8 nm. Calculate the mass concentration of zirconium in the total zirconium test solution and the total zirconium sample blank test solution using a binary linear equation corresponding to the calibration curve drawn with the standard solution in step S3. ρ2,

[0080]

[0081] Calculate ω according to the following formula:

[0082]

[0083] Where:

[0084] ω—mass fraction of zirconium oxide, in %;

[0085] ρ1—mass concentration of zirconium in the total zirconium test solution of the sample, in micrograms per milliliter (μg / mL);

[0086] —Mass concentration of zirconium in the blank solution of the total zirconium sample, in micrograms per milliliter (μg / mL);

[0087] m1—the mass of the total zirconium sample tested, in grams (g);

[0088] V1—total zirconium test solution volume of the sample, in milliliters (mL);

[0089] ρ2—mass concentration of zirconium element in the sample solid solution zirconium test solution, in micrograms per milliliter (μg / mL);

[0090] —Mass concentration of zirconium element in blank solution of solid solution zirconium sample, in micrograms per milliliter (μg / mL);

[0091] m2—the mass of the solid solution zirconium sample to be tested, in grams (g);

[0092] V2—volume of sample solid solution zirconium test solution, in milliliters (mL);

[0093] 1.3509—The coefficient for converting zirconium to zirconium oxide.

[0094] The calculations show that:

[0095]

[0096] In this embodiment, the microwave digestion instrument has programmable temperature, pressure and time control, can monitor pressure and temperature during the digestion process, and is used in conjunction with a clamping device, a protective device and a pressure relief device.

[0097] In this embodiment, an inductively coupled plasma atomic emission spectrometer is used, equipped with a hydrofluoric acid resistant atomization system and a peristaltic pump for sample injection. The recommended instrument operating parameters are shown in Table 1.

[0098] Table 1 Instrument working conditions

[0099]

[0100] in conclusion:

[0101] In this embodiment, the zirconium oxide content in the zirconium oxide dispersion strengthened platinum-rhodium alloy tested is 0.330%.

[0102] Example 2 Measurement of zirconium oxide content in platinum material

[0103] When the material to be tested is a dispersion-strengthened platinum material, the method for measuring the zirconium oxide content in the platinum material is the same as step 1 except that the sampling in step S1 is to accurately weigh 0.1 g of each sample; and the heating and dissolution in step S3 is to heat and dissolve on an electric heating plate.

[0104] According to the formula I = aρ + b, draw the calibration curve, see Figure 2 .

[0105]

[0106] It turns out that I = 8251.4ρ-142.57

[0107] The mass concentrations of zirconium in the total zirconium test solution, total zirconium sample blank test solution, solid solution zirconium test solution and solid solution zirconium blank test solution were calculated using a binary linear equation corresponding to the calibration curve drawn with the standard solution. ρ2,

[0108]

[0109] Calculate ω according to the formula:

[0110]

[0111]

[0112] Conclusion: The zirconium oxide content in the zirconium oxide dispersion strengthened platinum material tested in this example is 0.193%.

[0113] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs may also make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the present invention should also fall within the protection scope of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention. Other devices that are the same or similar to the above are all within the protection scope of the present invention.

Claims

1. A method for determining the content of zirconium oxide in a dispersion-strengthened platinum-based material, characterized in that: The steps include: 1) Take two samples of dispersion-strengthened platinum-based material, set the mass of sample 1 to m1 and the mass of sample 2 to m2, and keep them for later use; 2) Preparation of test solution: Prepare a total zirconium test solution and a total zirconium sample blank test solution; a solid solution zirconium test solution and a solid solution zirconium sample blank test solution; The specific steps for preparing the test solution are as follows: 2.1) Preparation of total zirconium test solution Add a mixture of hydrochloric acid and nitric acid and hydrofluoric acid to sample 1, heat to dissolve, cool to room temperature, and adjust the volume to 100 ml, record the volume as V1, and set aside; 2.2) Preparation of blank test solution for total zirconium sample Take a mixture of hydrochloric acid and nitric acid and hydrofluoric acid, heat and dissolve them, cool to room temperature, and dilute to 100 ml for later use; 2.3) Preparation of solid solution zirconium test solution Add a mixture of hydrochloric acid and nitric acid to sample 2, heat to dissolve, cool to room temperature, and after precipitation, adjust the volume to 100 ml, record the volume as V2, and set aside; 2.4) Preparation of blank test solution for solid solution zirconium sample Take a mixture of hydrochloric acid and nitric acid, heat to dissolve, cool to room temperature, and dilute to 100 ml for later use; 3) Calibration curve drawing: A standard solution with a zirconium content of 1000 μg / mL was selected to prepare a standard solution with a zirconium concentration of 100 μg / mL; 0.00 ml, 0.50 ml, 1.00 ml, 2.00 ml, 3.00 ml, 4.00 ml, 5.00 ml, and 10.00 ml of the zirconium standard solution were respectively added with a mixed acid of hydrochloric acid and nitric acid and hydrofluoric acid, wherein the volume ratio of the mixed acid to hydrofluoric acid was 10 to 5:1, and the solution was diluted to 100 ml with water, and shaken well to prepare a series of calibration solutions; The intensity of the zirconium element in the above series of calibration solutions was tested at a wavelength of 343.8 nm or 339.1 nm in the spectrometer, and a linear regression was performed with the intensity of the zirconium element as the ordinate and the mass concentration of zirconium in the calibration solution as the abscissa; 4) Calculation of zirconium element mass concentration in test solution: The emission intensity of zirconium element in the total zirconium test solution, the total zirconium sample blank test solution, the solid solution zirconium test solution and the solid solution zirconium sample blank test solution is tested at a spectrometer wavelength of 343.8 nm or 339.1 nm, and the mass concentration of zirconium element in the total zirconium test solution, the total zirconium sample blank test solution, the solid solution zirconium test solution and the solid solution zirconium sample blank test solution is calculated using the following formula corresponding to the calibration curve drawn with the standard solution in step 3): Where: ω—mass fraction of zirconium oxide, in %; ρ1—mass concentration of zirconium in the total zirconium test solution of the sample, in μg / mL; —Mass concentration of zirconium in the blank solution of the total zirconium sample, in μg / mL; m1—the mass of the total zirconium sample tested, in g; V1—total zirconium test solution volume of the sample, in mL; ρ2—mass concentration of zirconium element in the sample solid solution zirconium test solution, in μg / mL; —Mass concentration of zirconium element in blank solution of solid solution zirconium sample, in μg / mL; m2—the mass of the solid solution zirconium sample tested, in g; V2—volume of sample solid solution zirconium test solution, in mL; 1.3509—Coefficient for converting zirconium to zirconium oxide.

2. The assay method according to claim 1, wherein: Step 1) The particle size of the sample is less than 0.5 mm.

3. The assay method according to claim 1, wherein: The density of the nitric acid is 1.42 g / mL, the density of the hydrochloric acid is 1.19 g / mL, and the density of the hydrofluoric acid is 1.18 g / mL.

4. The assay method according to claim 1, wherein: The spectrometer is an inductively coupled plasma atomic emission spectrometer.

5. The assay method according to claim 1, wherein: The volume ratio of hydrochloric acid to nitric acid in the mixed acid is 3:

1.

6. The assay method according to claim 1, wherein: The volume ratio of the mixed acid to the hydrofluoric acid is 10:

1.

7. The assay method according to claim 1, wherein: In step 2.3), the precipitate is zirconium oxide.

8. The assay method according to claim 1, wherein: In the heating and dissolving of steps 2.3) and 2.4), if the material to be tested is a platinum-based alloy, electric heating and dissolving are adopted; if the material to be tested is a platinum-rhodium alloy, microwave digestion instrument is adopted for heating and dissolving.

Citation Information

Patent Citations

  • Method for measuring contents of zirconium and zirconia in strengthened dispersion platinum

    CN105466910A

  • Zirconium oxide dissolving method

    CN115784302A

Cited By

  • Rapid detection and analysis method for oxidation rate of active elements in alloy material