Negative electrode sheet and processing method thereof, battery and electronic device

By using a flexible cladding layer on the negative electrode sheet of the lithium battery, the stress accumulation problem caused by volume changes is solved, the battery capacity and life are improved, and the cost is reduced.

CN117133882BActive Publication Date: 2024-11-08HONOR DEVICE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310268791.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-10
Publication Date
2024-11-08
Estimated Expiration
2043-03-10

AI Technical Summary

Technical Problem

The negative electrode sheet of the existing lithium battery has internal stress accumulation due to the change in the volume of the silicon-based material during the charging and discharging process, which can easily lead to rupture and damage to the SEI film, which in turn affects the capacity and life of the battery.

Method used

A flexible cladding layer is used to coat silicon-based material particles with supramolecular polymers, adapting to volume changes through the fracture and generation of non-covalent bonds, alleviating internal stress, and improving the structural strength and binding force of the material layer through adhesive properties.

Benefits of technology

It effectively reduces the risk of rupture of the negative electrode plate during charging and discharging, improves the capacity and service life of the battery, and reduces material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117133882B_ABST
    Figure CN117133882B_ABST
Patent Text Reader

Abstract

The present application provides a negative electrode plate and a processing method thereof, a battery and an electronic device, and relates to the field of terminal technology. The negative electrode plate includes: a negative electrode current collector and a negative electrode polar material layer. The negative electrode polar material layer is arranged on the surface of the negative electrode current collector, and the negative electrode polar material layer includes active material particles, and the active material particles include a core and a flexible coating layer. The flexible coating layer wraps the core, and the material of the core includes silicon-based material particles, and the material of the flexible coating layer includes supramolecular polymers. During the charge and discharge process of the battery, the flexible coating layer can exert a certain restraining effect on the volume expansion of the core, and to a certain extent alleviate the internal stress generated by the change in the volume of the core, thereby reducing the risk of expansion and rupture of the core to a certain extent, and preventing the problem of excessive thickness and rapid capacity decay of the battery cell caused by the increase in the porosity of the negative electrode polar material layer and the loss of active material particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of terminal technology, and in particular to a negative electrode plate and a processing method thereof, a battery and an electronic device. Background Art

[0002] With the development of economy, electronic devices such as portable electronic products, drones, electric vehicles, etc. urgently need batteries with higher energy density, higher power density, longer cycle life and safer. However, the energy density of existing lithium batteries with graphite as negative electrode is close to the upper limit and cannot meet the endurance and standby requirements of users for the above electronic devices.

[0003] Silicon-based materials are active materials with a gram capacity far higher than that of graphite. In addition, silicon-based materials have many advantages, such as high volumetric capacity, moderate lithium insertion and extraction potential, abundant reserves, low price, environmental protection and non-toxicity. Therefore, silicon-based materials are an ideal choice to replace graphite materials in the negative electrode active material of batteries and improve the energy density of lithium batteries.

[0004] However, due to the huge volume effect of silicon-based materials, the volume change rate caused by its expansion / contraction is relatively large during the process of repeated lithium insertion and extraction (i.e., charging and discharging). Therefore, during the process of battery charging and discharging, it is easy to cause internal stress accumulation of silicon-based material particles, and eventually expand, rupture and pulverize. The silicon-based material particles are broken and the SEI film is damaged, so that the broken silicon-based material particles are in contact with the electrolyte, so a new SEI film will be regenerated at the damaged part of the SEI film, consuming the lithium ions in the electrolyte. In addition, the expansion and rupture of silicon-based material particles will also destroy the conductive network of the negative electrode, resulting in the inability of some active substances to participate in the reaction, resulting in capacity loss. At the same time, due to the volume deformation of the silicon-based material, the negative electrode polar material layer generates and accumulates a large stress, which causes the rupture of the negative electrode polar material layer, and then leads to the loss of electrical contact between the silicon-based material particles and between the silicon-based material particles and the current collector, and even part of the negative electrode polar material layer falls off from the current collector, resulting in an increase in the internal resistance of the battery and a loss of capacity. Summary of the invention

[0005] The embodiments of the present application provide a negative electrode plate and a processing method thereof, a battery and an electronic device.

[0006] To achieve the above objectives, the embodiments of the present application adopt the following technical solutions:

[0007] In a first aspect, a negative electrode sheet is provided, comprising: a negative electrode current collector and a negative electrode polar material layer. The negative electrode polar material layer is disposed on the surface of the negative electrode current collector, the negative electrode polar material layer comprises active material particles, the active material particles comprise a core and a flexible coating layer, the flexible coating layer wraps the core, the material of the core comprises silicon-based material particles, and the material of the flexible coating layer comprises a supramolecular polymer.

[0008] Since supramolecular polymers are a type of polymer connected by non-covalent bonds. The interaction of non-covalent bonds is reversible, that is, the non-covalent bonds in supramolecular polymers can be continuously broken and generated. Therefore, supramolecular polymers can respond to certain external stimuli, withdraw the stimulus, and restore the initial state. Since the flexible coating layer covers the silicon-based material particles, during the charging and discharging process, when the volume of the silicon-based material particles increases, the non-covalent bonds in the supramolecular polymer are continuously broken and regenerated, so that the flexible coating layer can adapt to the volume change of the silicon-based material particles and continuously produce tensile deformation. When the volume of the silicon-based material particles decreases, the non-covalent bonds in the supramolecular polymer are continuously broken and regenerated, so that the flexible coating layer can adapt to the volume change of the silicon-based material particles and continuously produce shrinkage deformation. Therefore, the flexible coating layer has excellent elastic deformation ability. In addition, the supramolecular polymer also has certain adhesive properties, so the flexible coating layer has certain adhesive ability.

[0009] In this way, during the charge and discharge process of the battery, the flexible coating layer can have a certain restraining effect on the volume expansion of the core, and to a certain extent alleviate the internal stress caused by the change in the volume of the core, thereby reducing the risk of the core expansion and rupture to a certain extent, and then reducing the risk of the conductive network of the negative electrode being destroyed. In addition, the flexible coating layer can also play a role in isolating the core and the electrolyte, thereby avoiding the problem of regeneration due to the rupture of the SEI film, avoiding the consumption of lithium ions, and being beneficial to improving the capacity and service life of the battery. In addition, it can also prevent the problem of large stress accumulation at the negative electrode polar material layer caused by the volume change of the core to a certain extent, thereby avoiding the rupture of the negative electrode polar material layer, and then avoiding the loss of electrical contact between silicon-based material particles and between silicon-based material particles and negative electrode current collectors, and the problem of part of the negative electrode polar material layer falling off from the negative electrode current collector, which is beneficial to improving the capacity and service life of the battery. In addition, since the supramolecular polymer has certain adhesive properties, in the negative electrode polar material layer, two adjacent active material particles and between the active material particles and the conductive additive are conducive to bonding with the help of the flexible coating layer, thereby improving the structural strength of the negative electrode polar material layer, and it is also beneficial to improve the bonding strength between the negative electrode polar material layer and the negative electrode current collector, thereby further preventing part of the negative electrode polar material layer from falling off from the negative electrode current collector, causing the problem of increased internal resistance and capacity loss of the battery.

[0010] In some embodiments of the first aspect, the silicon-based material particles include at least one of silicon particles, silicon dioxide particles, silicon monoxide particles, and silicon-carbon composite material particles. That is, the silicon-based material particles include one or more of silicon particles, silicon dioxide particles, silicon monoxide particles, and silicon-carbon composite material particles.

[0011] In some embodiments of the first aspect, the flexible coating layer is attached to the outer surface of the inner core, so that the structure is simple and easy to process and manufacture.

[0012] In some embodiments of the first aspect, because the supramolecular polymer connected by hydrogen bonds has excellent reversibility, the supramolecular polymer has the advantages of good film-forming property, elastic deformation ability and strong ductility. In addition, the hydrogen-bonded supramolecular polymer has good bonding properties. Therefore, the supramolecular polymer is a hydrogen-bonded supramolecular polymer.

[0013] In some embodiments of the first aspect, the flexible coating layer is formed of a supramolecular polymer, thereby making the material composition simple, easy to manufacture, and conducive to reducing costs, and conducive to improving the elastic deformation capacity and bonding performance of the flexible coating layer.

[0014] In some embodiments of the first aspect, the flexible coating layer may further include a conductive material. For example, the flexible coating layer is formed by mixing a supramolecular polymer and a conductive material. In this way, the flexible coating layer can be used to conduct electricity, so that a conductive network is formed between the core and the conductive additive, thereby improving the charge and discharge efficiency of the battery.

[0015] Exemplarily, the conductive material includes one or two or more of conductive carbon black, graphene, carbon nanotubes, and graphite.

[0016] In some embodiments of the first aspect, the peel strength of the flexible coating layer has a value range greater than or equal to 10N / m. As a result, the bonding strength between the flexible coating layer and the inner core is high, which is beneficial to improve the bonding strength between the active material particles and between the active material particles and the negative electrode current collector, thereby effectively preventing part of the negative electrode polar material layer from peeling off from the negative electrode current collector and entering the electrolyte during the charge and discharge process of the battery. Furthermore, it can avoid the problem of increased internal resistance and capacity loss of the battery caused by the cracking and peeling of part of the negative electrode polar material layer, and the loss of electrical contact between the silicon-based material particles and the negative electrode current collector, and even the fall-off of part of the negative electrode polar material layer from the negative electrode current collector, which is beneficial to improve the capacity and service life of the battery.

[0017] Exemplarily, the peel strength of the flexible covering layer has a value range of less than or equal to 20 N / m.

[0018] In some embodiments of the first aspect, the elastic modulus of the flexible coating layer ranges from 0.3 GPa to 8 GPa. Thus, the flexible coating layer has good elastic deformation capability.

[0019] Exemplarily, the elastic modulus of the flexible coating layer is 0.5 GPa, 0.6 GPa, 0.8 GPa, 0.9 GPa, 1 GPa, 1.2 GPa, 1.5 GPa, 1.7 GPa, 1.8 GPa, 2 GPa, 2.1 GPa, 2.5 GPa, 2.8 GPa, 3 GPa, 3.2 GPa, 3.5 GPa, 3.8 GPa, 4 GPa, 4.2 GPa, 4.5 GPa, 4.8 GPa, 5 GPa, 5.2 GPa, 5.5 GPa, 5.8 GPa, 6 GPa, 6.2 GPa, 6.5 GPa, 6.7 GPa, 7 GPa, 7.2 GPa, 7.5 GPa, or 7.8 GPa. Thus, it is beneficial to ensure the elastic deformation capacity of the flexible coating layer.

[0020] In some embodiments of the first aspect, the material forming the supramolecular polymer includes a first material and a second material. The first material includes a polymeric acid and / or a polymeric anhydride, wherein the polymeric anhydride is formed by dehydrating the polymeric acid; wherein the polymeric acid includes one or more of a monomeric fatty acid, a dimerized fatty acid, and a trimerized fatty acid. The second material includes a polyol and / or a polyamine. The supramolecular polymer formed by the first material and the second material has good elastic deformation ability and bonding performance, and the material is cheap and low in cost.

[0021] Exemplarily, the polyamine includes, but is not limited to, at least one of diethylenetriamine, triethylenetetramine, ethylenediamine, propylenetriamine, and the like.

[0022] Exemplarily, the polyol includes, but is not limited to, at least one of ethylene glycol, glycerol, and the like.

[0023] In some embodiments of the first aspect, when the weight of the second material is 1 part, the weight of the first material ranges from 2 parts to 10 parts. In this way, the ratio of the first material to the second material is reasonable, which is conducive to obtaining a supramolecular polymer with excellent elastic deformation ability and bonding performance.

[0024] For example, when the weight of the second material is 1 part, the weight of the first material ranges from 4 parts to 8 parts. In this way, the ratio of the first material to the second material is more reasonable, which is conducive to obtaining a supramolecular polymer with excellent elastic deformation ability and bonding performance.

[0025] In some embodiments of the first aspect, the negative electrode polar material layer further includes a conductive additive, and the negative electrode polar material layer is composed of the conductive additive and active material particles, thereby facilitating the reduction of material costs.

[0026] Specifically, the conductive additive includes at least one of a granular additive, a linear additive, and a flake additive.

[0027] In some embodiments of the first aspect, the conductive additive includes additives in the form of granular additives and linear additives; or, the conductive additive includes additives in the form of granular additives and flake additives; or, the conductive additive includes additives in the form of linear additives and flake additives; or, the conductive additive includes additives in the form of granular additives, linear additives and flake additives. In this way, conductive additives of different forms can complement each other, increase the contact area between the conductive additives, and improve the distribution density of the conductive additives in the negative electrode polar material layer, so that conductive additives of different forms can be used to construct a conductive network in the negative electrode polar material layer to form a conductive path. In addition, the mutual complementation between conductive additives of different forms increases the contact area, which is conducive to ensuring the conductivity of the negative electrode polar material layer under the premise of a lower amount of conductive additives. In addition, the mutual interlocking degree of conductive additives of different forms with the flexible coating layer is different. The use of conductive additives of different forms is conducive to compensating for the problem that the conductive additive of a single form cannot form a conductive path with the core due to the weak interlocking ability of the conductive additive with the flexible coating layer, and is more conducive to the construction of a conductive path between the core and the conductive additive in the active material particles.

[0028] In some embodiments of the first aspect, the linear additive includes carbon nanotubes and / or carbon fibers; the flaky additive includes flaky graphene and / or flaky graphite; and the granular additive includes carbon black and / or graphite.

[0029] In some embodiments of the first aspect, the ratio of the equivalent diameter of the active material particles to the equivalent diameter of the inner core is greater than 1 and less than or equal to 1.3. This helps to limit the thickness of the flexible coating layer within a reasonable range, which helps to ensure the elastic deformation capacity and bonding performance of the flexible coating layer on the one hand, and the structural strength of the flexible coating layer on the other hand.

[0030] In some embodiments of the first aspect, the equivalent diameter of the core is nanometer-scale. In this way, compared with a core of a large size, it is beneficial to reduce the volume effect of the core during the battery charging and discharging process, facilitate the uniform distribution of more active material particles in the negative electrode polar material layer, and improve the battery charging and discharging efficiency.

[0031] In some embodiments of the first aspect, the equivalent diameter of the core is in micrometer order. That is, the equivalent diameter of the core is greater than or equal to 1 micrometer (um) and less than 1000um. This is more conducive to forming a flexible coating layer on the core and improving the bonding strength between the flexible coating layer and the core.

[0032] In some embodiments of the first aspect, the equivalent diameter of the kernel is in the range of 10nm to 30um. In this way, on the one hand, it is conducive to preventing the problem that the equivalent diameter of the kernel is set too small, which is not conducive to forming a flexible coating on the surface of the kernel and the bonding strength between the flexible coating and the kernel is weak. On the other hand, it is conducive to preventing the problem that the volume change of the kernel during the charge and discharge process is too large due to the size of the kernel being set too large. That is, the equivalent diameter of the kernel is in the range of 10nm to 30um, which makes the size design of the kernel more reasonable, which can not only ensure the connection strength between the flexible coating and the kernel, but also reduce the volume change of the kernel during the charge and discharge process of the battery, which is convenient for evenly distributing more active material particles in the negative electrode polar material layer, and improving the charge and discharge efficiency of the battery.

[0033] In a second aspect, the present application provides a battery, comprising: a positive electrode plate, a separator and a negative electrode plate; wherein the negative electrode plate is the negative electrode plate in any of the above technical solutions, and the positive electrode plate and the negative electrode plate are separated by a separator.

[0034] In a third aspect, the present application provides an electronic device, comprising: an electrical device and a battery, wherein the battery is the battery in the above embodiment. The battery is electrically connected to the electrical device.

[0035] Among them, the technical effects brought about by any design method in the second aspect to the third aspect can refer to the technical effects brought about by different design methods in the first aspect, and will not be repeated here.

[0036] In a fourth aspect, the present application can provide a method for processing a negative electrode plate, the processing method comprising: setting a negative electrode polar material layer on the surface of the negative electrode current collector; wherein the negative electrode polar material layer comprises active material particles, the active material particles comprise an inner core and a flexible coating layer, the flexible coating layer wraps the inner core, the material of the inner core comprises silicon-based material particles, and the material of the flexible coating layer comprises a supramolecular polymer.

[0037] Since supramolecular polymers are a type of polymer connected by non-covalent bonds. The interaction of non-covalent bonds is reversible, that is, the non-covalent bonds in supramolecular polymers can be continuously broken and generated. Therefore, supramolecular polymers can respond to certain external stimuli, withdraw the stimulus, and restore the initial state. Since the flexible coating layer covers the silicon-based material particles, during the charging and discharging process, when the volume of the silicon-based material particles increases, the non-covalent bonds in the supramolecular polymer are continuously broken and regenerated, so that the flexible coating layer can adapt to the volume change of the silicon-based material particles and continuously produce tensile deformation. When the volume of the silicon-based material particles decreases, the non-covalent bonds in the supramolecular polymer are continuously broken and regenerated, so that the flexible coating layer can adapt to the volume change of the silicon-based material particles and continuously produce shrinkage deformation. Therefore, the flexible coating layer has excellent elastic deformation ability. In addition, the supramolecular polymer also has certain adhesive properties, so the flexible coating layer has certain adhesive ability.

[0038] The negative electrode sheet prepared by the above method can have a certain restraining effect on the volume expansion of the core during the charge and discharge process of the battery, and alleviate the internal stress caused by the change in the volume of the core to a certain extent, thereby reducing the risk of the core expansion and rupture to a certain extent, and then reducing the risk of the conductive network of the negative electrode being destroyed. In addition, the flexible coating layer can also play a role in isolating the core and the electrolyte, thereby avoiding the problem of regeneration due to the rupture of the SEI film, avoiding the consumption of lithium ions, and being beneficial to improving the capacity and service life of the battery. In addition, it can also prevent the problem of large stress accumulation at the negative electrode polar material layer caused by the volume change of the core to a certain extent, thereby avoiding the rupture of the negative electrode polar material layer, and then avoiding the loss of electrical contact between silicon-based material particles and between silicon-based material particles and negative electrode current collectors, and the problem of part of the negative electrode polar material layer falling off from the negative electrode current collector, which is beneficial to improving the capacity and service life of the battery. In addition, since the supramolecular polymer has certain adhesive properties, in the negative electrode polar material layer, two adjacent active material particles and between the active material particles and the conductive additive are conducive to bonding with the help of the flexible coating layer, thereby improving the structural strength of the negative electrode polar material layer, and it is also beneficial to improve the bonding strength between the negative electrode polar material layer and the negative electrode current collector, thereby further preventing part of the negative electrode polar material layer from falling off from the negative electrode current collector, causing the problem of increased internal resistance and capacity loss of the battery.

[0039] In some embodiments of the fourth aspect, because the supramolecular polymer connected by hydrogen bonds has excellent reversibility, the supramolecular polymer has the advantages of good film-forming property, elastic deformation ability and strong ductility. In addition, the hydrogen-bonded supramolecular polymer has good adhesive properties. Therefore, the supramolecular polymer is a hydrogen-bonded supramolecular polymer.

[0040] In some embodiments of the fourth aspect, a negative electrode polar material layer is provided on the surface of the negative electrode current collector, comprising: heating a first material and a second material under a protective gas atmosphere so that the first material and the second material react to obtain a supramolecular polymer slurry; providing the supramolecular polymer slurry on the outer surface of the inner core to form active material particles having a flexible coating layer; fully mixing the active material particles and the conductive additive to obtain a polar slurry; providing the polar slurry on the surface of the negative electrode current collector to obtain a negative electrode polar material layer. In this way, the forming material of the flexible coating layer is only a supramolecular polymer, that is, the flexible coating layer is formed by a single supramolecular polymer material. In this way, the material composition is simple, easy to make, conducive to reducing costs, and conducive to improving the elastic deformation ability and bonding performance of the flexible coating layer. In addition, the negative electrode polar material layer is formed by the conductive additive and the active material particles, which saves the setting of the adhesive and is conducive to reducing material costs. In addition, the negative electrode polar material layer can be closely attached to the negative electrode current collector, which can improve the bonding strength between the negative electrode polar material layer and the negative electrode current collector. This method is simple, the conditions are easy to control, and it is suitable for industrial production.

[0041] In some embodiments of the fourth aspect, a negative electrode polar material layer is provided on the surface of the negative electrode current collector, comprising: heating the first material and the second material under a protective gas atmosphere so that the first material and the second material react to obtain a supramolecular polymer slurry; providing the supramolecular polymer slurry on the surface of the inner core to form active material particles having a flexible coating layer; fully mixing the active material particles, the conductive additive and the solvent to obtain a polar slurry; providing the polar slurry on the surface of the negative electrode current collector; drying the polar slurry on the negative electrode current collector so that the solvent in the polar slurry evaporates to obtain the negative electrode polar material layer. In this way, the forming material of the flexible coating layer is only the supramolecular polymer, that is, the flexible coating layer is formed by a single supramolecular polymer material. In this way, the material composition is simple, easy to make, conducive to reducing costs, and conducive to improving the elastic deformation capacity and bonding performance of the flexible coating layer. In addition, the negative electrode polar material layer is formed by conductive additives and active material particles, which saves the setting of the adhesive and helps to reduce material costs. Moreover, the negative electrode polar material layer can be closely attached to the negative electrode current collector, which can improve the bonding strength between the negative electrode polar material layer and the negative electrode current collector. This method is simple, the conditions are easy to control, and it is suitable for industrial production.

[0042] In some embodiments of the fourth aspect, the solvent comprises at least one of water, ethanol, and NMP (N-Methylpyrrolidone).

[0043] In some embodiments of the fourth aspect, the first material includes a polymeric acid and / or a polymeric anhydride, wherein the polymeric anhydride is formed by dehydrating the polymeric acid; wherein the polymeric acid includes one or more of a monomeric fatty acid, a dimerized fatty acid, and a trimerized fatty acid. The second material includes a polyol and / or a polyamine. The supramolecular polymer formed by the first material and the second material has good elastic deformation ability and bonding performance, and the material is cheap and low in cost.

[0044] Exemplarily, the polyamine includes, but is not limited to, at least one of diethylenetriamine, triethylenetetramine, ethylenediamine, propylenetriamine, and the like.

[0045] Exemplarily, the polyol includes, but is not limited to, at least one of ethylene glycol, glycerol, and the like.

[0046] In some embodiments of the fourth aspect, the peel strength of the flexible coating layer has a value range greater than or equal to 10N / m. As a result, the bonding strength between the flexible coating layer and the inner core is high, which is beneficial to improve the bonding strength between the active material particles and between the active material particles and the negative electrode current collector, thereby effectively preventing part of the negative electrode polar material layer from peeling off from the negative electrode current collector and entering the electrolyte during the charge and discharge process of the battery. Furthermore, it can avoid the problem of increased internal resistance and capacity loss of the battery caused by the cracking and peeling of part of the negative electrode polar material layer, and the loss of electrical contact between the silicon-based material particles and the negative electrode current collector, and even the fall-off of part of the negative electrode polar material layer from the negative electrode current collector, which is beneficial to improve the capacity and service life of the battery.

[0047] Exemplarily, the peel strength of the flexible covering layer has a value range of less than or equal to 20 N / m.

[0048] In some embodiments of the fourth aspect, the elastic modulus of the flexible coating layer ranges from 0.3 GPa to 8 GPa. Thus, the flexible coating layer has good elastic deformation capability.

[0049] In some embodiments of the fourth aspect, the supramolecular polymer slurry is disposed on the surface of the inner core to form active material particles with a flexible coating layer, including: disposing the supramolecular polymer slurry on the surface of the inner core to cover the surface of the inner core with the supramolecular polymer slurry; heating the supramolecular polymer slurry on the surface of the inner core for a second preset time at a second preset temperature; and cooling the supramolecular polymer slurry to form a flexible coating layer. Since the inner core includes silicon-based material particles, the surface of the silicon-based material particles has silicon-oxygen bonds, heating the supramolecular polymer slurry on the surface of the inner core is, on the one hand, conducive to improving the fluidity and diffusivity of the supramolecular polymer slurry, thereby improving the wetting effect between the supramolecular polymer slurry and the surface of the inner core, and on the other hand, it is conducive to the non-covalent bonds in the supramolecular polymer to bond with the silicon-oxygen bonds after breaking, thereby improving the bonding strength between the flexible coating layer and the inner core through these two aspects.

[0050] In some embodiments of the fourth aspect, the second preset temperature is in the range of 70° C. to 120° C. and / or the second preset time is in the range of 3 min to 100 min. This helps to ensure that the non-covalent bonds in the supramolecular polymer are bonded to the silicon-oxygen bonds after breaking.

[0051] In some embodiments of the fourth aspect, the second preset temperature is in the range of 90° C. to 110° C. This is conducive to ensuring that the non-covalent bonds in the supramolecular polymer are bonded to the silicon-oxygen bonds after being broken.

[0052] In some embodiments of the fourth aspect, the second preset time ranges from 3 minutes to 10 minutes, which is helpful to ensure that the non-covalent bonds in the supramolecular polymer are bonded to the silicon-oxygen bonds after being broken.

[0053] In some embodiments of the fourth aspect, the supramolecular polymer slurry is disposed on the surface of the inner core to cover the surface of the inner core with the supramolecular polymer slurry, comprising: disposing the supramolecular polymer slurry on the surface of the inner core at a third preset temperature to cover the surface of the inner core with the supramolecular polymer slurry; wherein the third preset temperature is greater than room temperature and less than the second preset temperature. The supramolecular polymer slurry is cooled. Thus, the supramolecular polymer slurry is disposed on the surface of the inner core at the third preset temperature, which is beneficial to improving the fluidity and diffusivity of the supramolecular polymer slurry, thereby improving the wetting effect between the supramolecular polymer slurry and the surface of the inner core, and further improving the bonding strength between the coating layer and the inner core.

[0054] Exemplarily, the third preset temperature ranges from 40°C to 50°C.

[0055] In some embodiments of the fourth aspect, when the weight of the second material is 1 part, the weight of the second material ranges from 2 parts to 10 parts. This is conducive to obtaining a supramolecular polymer with excellent elastic deformation ability and adhesive properties.

[0056] In some embodiments of the fourth aspect, when the weight of the second material is 1 part, the weight of the second material ranges from 4 parts to 8 parts. This is conducive to obtaining a supramolecular polymer with excellent elastic deformation ability and adhesive properties.

[0057] In some embodiments of the fourth aspect, the conductive additive includes additives in the form of granular additives and linear additives; or, the conductive additive includes additives in the form of granular additives and flake additives; or, the conductive additive includes additives in the form of linear additives and flake additives; or, the conductive additive includes additives in the form of granular additives, linear additives and flake additives. In this way, conductive additives of different forms can complement each other, increase the contact area between the conductive additives, and improve the distribution density of the conductive additives in the negative electrode polar material layer, so that conductive additives of different forms can be used to construct a conductive network in the negative electrode polar material layer to form a conductive path. In addition, the mutual complementation between conductive additives of different forms increases the contact area, which is conducive to ensuring the conductivity of the negative electrode polar material layer under the premise of a lower amount of conductive additives. In addition, the degree of mutual interlocking between conductive additives of different forms and the flexible coating layer is different. The use of conductive additives of different forms is conducive to compensating for the problem that the conductive additive of a single form cannot form a conductive path with the core due to the weak interlocking ability of the conductive additive with the flexible coating layer, and is more conducive to the construction of a conductive path between the core and the conductive additive in the active material particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 Various structural diagrams of electronic devices provided in some embodiments of the present application;

[0059] Figure 2 A front view of a battery provided in some embodiments of the present application;

[0060] Figure 3 Based on Figure 2 The schematic diagram of the cross-sectional structure of the battery shown at line AA;

[0061] Figure 4 Based on Figure 3 A schematic diagram of the cross-sectional structure of the positive electrode sheet in the battery shown;

[0062] Figure 5 Based on Figure 3 A schematic diagram of the cross-sectional structure of the negative electrode sheet in the battery shown;

[0063] Figure 6 A schematic diagram of another negative electrode sheet provided in an embodiment of the present application;

[0064] Figure 7 Based on Figure 6 Schematic diagram of volume change of active material particles in the negative electrode sheet during charge and discharge process;

[0065] Figure 8 A flow chart of a method for processing a negative electrode sheet provided in an embodiment of the present application;

[0066] Fig. 9 Based on Figure 8 A specific flow chart of step S10 in the negative electrode sheet processing method shown;

[0067] Fig.10 Based on Fig. 9 The specific flow chart of step S12 in the negative electrode sheet processing method shown;

[0068] Fig.11 Based on Fig.10 The specific flow chart of step S121 in the negative electrode sheet processing method shown;

[0069] Fig.12 Based on Figure 8 Another specific flow chart of step S10 in the method for processing a negative electrode sheet is shown. DETAILED DESCRIPTION

[0070] In the embodiments of the present application, the terms "exemplary" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "exemplary" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "exemplary" or "for example" is intended to present related concepts in a specific way.

[0071] In the embodiments of the present application, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0072] In the description of the embodiments of the present application, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, at least one of a, b, or c can represent: a, b, c, ab, ac, bc, or abc, where a, b, and c can be single or multiple.

[0073] In the description of the embodiments of the present application, the term "and / or" refers to and covers any and all possible combinations of one or more of the associated listed items. The term "and / or" is a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in the present application generally indicates that the associated objects before and after are in an "or" relationship.

[0074] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, "connection" can be a detachable connection or a non-detachable connection; it can be a direct connection or an indirect connection through an intermediate medium.

[0075] In the description of the embodiments of the present application, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the statement "comprises a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element. In the absence of further restrictions, an element defined by the statement "comprises a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element.

[0076] Before introducing the embodiments of the present application, the lithium battery and some professional terms to be mentioned in the embodiments of the present application are first introduced, specifically:

[0077] Working principle of lithium battery: The process of charging and discharging of lithium battery is the process of lithium ions moving between the positive and negative electrodes. Specifically, during the charging process of the battery, the lithium atoms (Li) in the positive electrode (i.e., the positive electrode below) decompose into lithium ions (Li + ) and electron (e - ). Electronic (e -) reaches the negative electrode (i.e., the negative electrode plate hereinafter) through the external circuit. + ) escapes from the positive electrode lattice and passes through the electrolyte and the separator to the negative electrode. + ) at the negative electrode and the electrons (e - ) to form lithium atoms (Li). The discharge process of lithium batteries is the opposite of the charging process. The lithium atoms (Li) on the negative electrode lose electrons (e - ) to form lithium ions (Li + ). The electrons reach the positive electrode through the external circuit. Lithium ions (Li + ) is released from the negative electrode lattice and passes through the electrolyte and the separator to the positive electrode. + ) at the positive electrode and electrons (e - ) to form lithium atoms.

[0078] Solid electrolyte interface (SEI) film: a passivation film with solid electrolyte properties. Specifically, during the first charge and discharge process of a lithium battery, the electrode material and the electrolyte react at the solid-liquid interface to form a passivation film covering the surface of the electrode material. This passivation film is an excellent conductor of lithium ions, allowing lithium ions to be transported, embedded and removed freely. It is worth noting that the formation of the SEI film will consume some lithium ions, increasing the irreversible capacity of the first charge and discharge. The SEI film is insoluble in organic solvents, can exist stably in organic electrolyte solutions, and solvent molecules cannot pass through this passivation film, thereby effectively preventing the co-embedding of solvent molecules.

[0079] Gram capacity: The ratio of the capacity that can be released by the active material inside the battery to the mass of the active material.

[0080] Specific capacity: There are two types of specific capacity: one is the mass specific capacity, which is the amount of electricity that can be discharged by unit mass of the battery or active material; the other is the volume specific capacity, which is the amount of electricity that can be discharged by unit volume of the battery or active material.

[0081] Supramolecular polymer: It is an array polymer in which repeating units are connected by reversible and directional non-covalent bond interactions. Supramolecular polymers can be formed based on a variety of intermolecular interactions and their synergistic or multiple interactions, such as hydrogen bonds, coordination effects, host-guest interactions, charge transfer interactions, π-π interactions, etc. Supramolecular polymers can be mainly divided into hydrogen bond type supramolecular polymers, complex type supramolecular polymers, π-π type supramolecular polymers, and hybrid supramolecular polymers according to the different non-covalent bond forces. Among them, hybrid supramolecular polymers contain multiple non-covalent bond forces.

[0082] Cross-linked structure: Cross-linked structure refers to a macromolecule in which linear polymer chains are connected by branches or chemical bonds to form a three-dimensional network structure.

[0083] Straight chain structure: A straight chain structure is a structure without branches.

[0084] Secondary battery: also known as rechargeable battery or storage battery, refers to a battery that can be recharged to activate the active material after the battery is discharged and continue to be used.

[0085] The present application provides an electronic device. The electronic device is a type of electronic device including a battery 10. Figure 1 , Figure 1 The electronic device 100 of some embodiments of the present application is provided in various structural forms. Specifically, the electronic device 100 includes but is not limited to a mobile phone 100A, a tablet personal computer 100B, a laptop computer, a personal digital assistant (PDA), a personal computer, a notebook computer 100C and other portable electronic products, an electric toothbrush 100E, a sweeping robot 100D, a mobile power supply 100F, a drone, an electric car, etc.

[0086] The electronic device 100 further includes electrical components, including but not limited to at least one of display screen, speaker, camera, flash, receiver, main board, sub-board, sensor and other electronic components. The battery 10 is electrically connected to the electrical components to supply power to the electrical components.

[0087] See also Figure 2 and Figure 3 , Figure 2 A front view of a battery 10 provided in some embodiments of the present application, Figure 3 Based on Figure 2 The cross-sectional structure diagram of the battery 10 at the AA line is shown. In this embodiment, the battery 10 is a secondary battery. Specifically, the battery 10 is a secondary lithium battery. The battery 10 includes a housing 2, an electrolyte 3 and a battery cell 1.

[0088] Understandably, Figure 2 and Figure 3 The following figures and the related drawings only schematically show some components of the battery 10, and the actual shapes, sizes, positions and structures of these components are not limited to Figure 2 and Figure 3 and the accompanying drawings below.

[0089] The shell 2 is used to encapsulate and protect the electrolyte 3 and the battery cell 1. The shape of the shell 2 includes but is not limited to a cuboid, a cylinder or a truncated cone.

[0090] The material of the shell 2 can be metal, such as steel, copper or aluminum, or a composite film. When the material of the shell 2 is a composite film. Specifically, the composite film is divided into at least three layers, the middle layer is a metal coating layer, which plays a role in isolating moisture, the outer layer is a plastic coating layer, which plays a role in preventing the penetration of air, especially oxygen; the inner layer is a sealing layer, which plays a role in sealing and preventing the electrolyte 3 from corroding the metal coating layer. The material of the sealing layer is selected from at least one of polyethylene, polypropylene, esters of polyethylene or polypropylene, and ion crosslinked products of polyethylene or polypropylene, and the polyethylene is selected from low-density polyethylene, medium-density polyethylene or high-density polyethylene; the polypropylene is selected from homopolymer polypropylene, block polypropylene or random polypropylene. The material of the metal coating layer is selected from at least one of metal, metal alloy, metal oxide or ceramic, and the metal is selected from aluminum, iron, silver, copper, nickel, manganese, tin, titanium, zirconium or vanadium; the material of the plastic coating layer is selected from at least one of polyamide resin, polyolefin, polycarbonate or fluororesin. The composite film can specifically be an aluminum-plastic film, wherein the middle layer of the aluminum-plastic film is an aluminum layer, which serves to isolate moisture, and the outer layer of the aluminum-plastic film is polyamide, which serves to prevent the penetration of air, especially oxygen; the inner layer of the aluminum-plastic film is a polypropylene layer, which serves to seal and prevent the electrolyte 3 from corroding the aluminum layer.

[0091] The electrolyte 3 is encapsulated in the housing 2. The electrolyte 3 is a carrier for transmitting lithium ions in the battery 10. The electrolyte 3 is generally prepared from raw materials such as high-purity organic solvents, electrolyte lithium salts, and necessary additives under certain conditions and in a certain proportion.

[0092] The battery cell 1 is disposed in the housing 2 and immersed in the electrolyte 3. Figure 3 The battery cell 1 includes a positive electrode sheet 12, a negative electrode sheet 11 and a separator 13. The positive electrode sheet 12 and the negative electrode sheet 11 are separated by the separator 13.

[0093] In some embodiments, please refer to Figure 3 , the battery cell 1 can be a wound structure. The battery cell 1 is formed by winding a diaphragm. Specifically, the diaphragm includes two diaphragms 13 (i.e., a first diaphragm and a second diaphragm). The diaphragm is formed by stacking a positive electrode sheet 12, a first diaphragm, a negative electrode sheet 11, and a second diaphragm in sequence. The positive electrode sheet 12 and the negative electrode sheet 11 can be separated by a diaphragm 13 to play an insulating isolation role to prevent short circuits between the two electrodes.

[0094] In other examples, the battery cell 1 may also be a laminated structure. Specifically, the positive electrode sheets 12 and the negative electrode sheets 11 are alternately and stacked in sequence, and a diaphragm 13 is provided between adjacent positive electrode sheets 12 and negative electrode sheets 11. The diaphragm 13 serves as an insulating barrier. The diaphragm 13 may be a diaphragm bag, a diaphragm 13 folded in a Z shape, or a plurality of single-piece diaphragms 13. The present application does not limit the specific structural form of the diaphragm 13 in the laminated battery cell 1, as long as it can insulate and isolate the positive electrode sheets 12 and the negative electrode sheets 11.

[0095] For example, the material of the separator 13 may be a polyolefin porous membrane.

[0096] See also Figure 4 , Figure 4 Based on Figure 3 The cross-sectional structure diagram of the positive electrode sheet 12 in the battery 10 is shown. The positive electrode sheet 12 includes a positive electrode current collector 121 and a positive electrode polar material layer 122 disposed on the surface of the positive electrode current collector 121.

[0097] Specifically, the positive electrode polar material layer 122 may be disposed on one side surface of the positive electrode current collector 121 in the thickness direction, or may be disposed on both side surfaces of the positive electrode current collector 121 in the thickness direction.

[0098] The positive electrode current collector 121 is used to collect current. The forming material of the positive electrode current collector 121 is aluminum (chemical formula: Al). The positive electrode polar material layer 122 is a material that participates in the charge and discharge reaction. The material of the positive electrode polar material layer 122 includes lithium compounds. Among them, the lithium compound includes but is not limited to lithium iron phosphate (chemical formula: LiFePO4), lithium nickelate (chemical formula: Li x NiO2), lithium cobalt oxide (chemical formula: Li x CoO2), lithium manganate (chemical formula: Li x MnO4) and a ternary material, illustratively, the ternary material is selected from a ternary material with a grade of NCM811, NCM622, NCM523, NCM111 or NCA.

[0099] See also Figure 5 , Figure 5 Based on Figure 3 The cross-sectional structure diagram of the negative electrode sheet 11 in the battery 10 is shown. The negative electrode sheet 11 includes a negative electrode current collector 111 and a negative electrode polar material layer 112 disposed on the surface of the negative electrode current collector 111.

[0100] Specifically, the negative electrode polar material layer 112 may be disposed on one side surface of the negative electrode current collector 111 in the thickness direction, or may be disposed on both side surfaces of the negative electrode current collector 111 in the thickness direction.

[0101] The negative electrode current collector 111 is used to collect current. The negative electrode current collector 111 is formed of copper (chemical formula: Cu). The negative electrode polar material layer 112 is a material that participates in charge and discharge reactions.

[0102] Generally, the negative electrode polar material layer 112 is made of a conductive additive, a negative electrode active material and a binder.

[0103] Silicon-based materials are active materials with a gram capacity far higher than that of graphite. In addition, silicon-based materials have many advantages, such as high volumetric capacity, moderate lithium insertion and extraction potential, abundant reserves, low price, environmental protection and non-toxicity. Therefore, when selecting negative electrode active materials, silicon-based material particles are an ideal choice. In other words, negative electrode active materials usually include silicon-based material particles.

[0104] However, due to the huge volume effect of silicon-based materials, the volume change rate caused by its expansion / contraction is relatively large during the process of repeated lithium insertion and extraction (i.e., charging and discharging). Therefore, during the charging and discharging process of the battery 10, it is easy to cause stress accumulation inside the silicon-based material particles, and finally expand, rupture and pulverize. The rupture and pulverization of the silicon-based material particles also cause damage to the SEI film, so that the ruptured silicon-based material particles are in contact with the electrolyte, so a new SEI film will be regenerated at the damaged part of the SEI film, consuming the lithium ions in the electrolyte. In addition, the expansion and rupture of the silicon-based material particles will also destroy the conductive network of the negative electrode, resulting in the inability of some active substances to participate in the reaction, resulting in capacity loss. At the same time, due to the volume deformation of the silicon-based material, the negative electrode polar material layer 112 generates and accumulates a large stress, causing the rupture of the negative electrode polar material layer 112, which in turn causes the loss of electrical contact between the silicon-based material particles and between the silicon-based material particles and the current collector, and even part of the negative electrode polar material layer 112 falls off from the current collector, causing the internal resistance of the battery 10 to increase and the capacity to lose.

[0105] To solve the above technical problems, please refer to Figure 6 , Figure 6 A schematic diagram of another negative electrode sheet 11 provided in an embodiment of the present application. The negative electrode sheet 11 is applied to the battery cell 1 of the battery 10 described above.

[0106] The negative electrode sheet 11 in this embodiment includes a negative electrode current collector 111 and a negative electrode polar material layer 112 disposed on the surface of the negative electrode current collector 111 .

[0107] The material of the negative electrode current collector 111 in this embodiment is the same as that of the negative electrode current collector 111 in the above embodiment.

[0108] Specifically, the negative electrode polar material layer 112 may be disposed on one side surface of the negative electrode current collector 111 in the thickness direction, or may be disposed on both side surfaces of the negative electrode current collector 111 in the thickness direction.

[0109] The negative polar material layer 112 includes active material particles 1121 and a conductive additive 1122 .

[0110] Please continue reading Figure 6 The active material particle 1121 includes a core 11212 and a flexible covering layer 11211 .

[0111] The material of the core 11212 includes silicon-based material particles. Exemplarily, the core 11212 is silicon-based material particles, that is, the core 11212 only includes silicon-based material particles and does not include other materials. Exemplarily, in addition to silicon-based material particles, the core 11212 may also include other materials, such as graphite particles.

[0112] Specifically, the silicon-based material particles include at least one of silicon particles, silicon dioxide particles, silicon monoxide particles, and silicon-carbon composite material particles. That is, the silicon-based material particles include one or more of silicon particles, silicon dioxide particles, silicon monoxide particles, and silicon-carbon composite material particles.

[0113] Exemplarily, the silicon-based material particles are silicon particles, silicon dioxide particles, silicon monoxide particles, or silicon-carbon composite material particles.

[0114] In another exemplary embodiment, the silicon-based material particles include two or more of silicon particles, silicon dioxide particles, silicon monoxide particles and silicon-carbon composite material particles. For example, the silicon-based material particles include silicon particles and silicon dioxide particles. Alternatively, the silicon-based material particles include silicon particles and silicon monoxide particles. Alternatively, the silicon-based material particles include silicon particles and silicon-carbon composite material particles. Alternatively, the silicon-based material particles include silicon particles, silicon dioxide particles and silicon monoxide particles. Alternatively, the silicon-based material particles include silicon particles, silicon dioxide particles and silicon-carbon composite material particles. Alternatively, the silicon-based material particles include silicon particles, silicon dioxide particles, silicon monoxide particles and silicon-carbon composite material particles. Alternatively, the silicon-based material particles include silicon particles, silicon dioxide particles, silicon monoxide particles and silicon-carbon composite material particles.

[0115] The flexible coating layer 11211 wraps the inner core 11212. For example, the flexible coating layer 11211 adheres to and wraps the outer surface of the inner core 11212, so that the structure is simple and easy to process and manufacture. In another exemplary embodiment, the flexible coating layer 11211 wraps the inner core 11212, and one or more flexible wrapping layers wrapping the inner core 11212 can be further arranged between the flexible coating layer 11211 and the inner core 11212.

[0116] The material of the flexible coating layer 11211 includes supramolecular polymers. Since supramolecular polymers are a type of polymers connected by non-covalent bonds, the interaction of non-covalent bonds is reversible, that is, the non-covalent bonds in the supramolecular polymers can be continuously broken and generated. Therefore, the supramolecular polymers can respond to certain external stimuli, and can return to the initial state when the stimuli are withdrawn. For details, please refer to Figure 7 , Figure 7 Based on Figure 6 Schematic diagram of the volume change of the active material particles 1121 in the negative electrode plate 11 shown in the charging and discharging process. Since the flexible coating layer 11211 covers the silicon-based material particles, during the charging and discharging process, when the volume of the silicon-based material particles increases, the non-covalent bonds J in the supramolecular polymer are constantly broken and regenerated, so that the flexible coating layer 11211 can adapt to the volume change of the silicon-based material particles and continuously produce tensile deformation. When the volume of the silicon-based material particles decreases, the non-covalent bonds J in the supramolecular polymer are constantly broken and regenerated, so that the flexible coating layer 11211 can adapt to the volume change of the silicon-based material particles and continuously produce shrinkage deformation. Therefore, the flexible coating layer 11211 has excellent elastic deformation ability. In addition, the supramolecular polymer also has certain bonding properties, so that the flexible coating layer 11211 has certain bonding ability.

[0117] In this way, during the charge and discharge process of the battery 10, the flexible coating layer 11211 can have a certain restraining effect on the volume expansion of the core 11212, and to a certain extent alleviate the internal stress caused by the volume change of the core 11212, thereby reducing the risk of expansion and rupture of the core 11212 to a certain extent, and further reducing the risk of damage to the conductive network of the negative electrode. In addition, the flexible coating layer 11211 can also play a role in isolating the core 11212 and the electrolyte 3, thereby avoiding the problem of regeneration due to the rupture of the SEI film, avoiding the consumption of lithium ions, and being beneficial to improving the capacity and service life of the battery. In addition, it can also prevent the problem of large stress accumulation at the negative electrode polar material layer 112 caused by the volume change of the core 11212 to a certain extent, thereby avoiding the rupture of the negative electrode polar material layer 112, and further avoiding the loss of electrical contact between the silicon-based material particles and between the silicon-based material particles and the negative electrode current collector 111, and the problem of part of the negative electrode polar material layer 112 falling off from the negative electrode current collector 111, which is beneficial to improving the capacity and service life of the battery 10. In addition, since the supramolecular polymer has a certain adhesive property, in the negative electrode polar material layer 112, two adjacent active material particles 1121 and between the active material particles 1121 and the conductive additive are advantageously bonded (combined) with the flexible coating layer 11211. Figure 6), improve the structural strength of the negative electrode polar material layer 112, and also help to improve the bonding strength between the negative electrode polar material layer 112 and the negative electrode current collector 111, thereby further preventing part of the negative electrode polar material layer 112 from falling off the negative electrode current collector 111, which would cause the problem of increased internal resistance and capacity loss of the battery 10, and also help to use supramolecular polymers to replace the adhesive in the above embodiment, thereby omitting the setting of the adhesive and reducing material costs.

[0118] In some embodiments, the supramolecular polymer is a hydrogen-bonded supramolecular polymer. That is to say, the non-covalent bonding method used in the supramolecular polymer includes hydrogen bonding. For example, the non-covalent bonding method used in the supramolecular polymer is only hydrogen bonding. Because the supramolecular polymer connected by hydrogen bonding has excellent reversibility, this type of supramolecular polymer has the advantages of good film-forming property, elastic deformation ability and strong ductility. In addition, the hydrogen-bonded supramolecular polymer has good bonding performance. When the supramolecular polymer is a hydrogen-bonded supramolecular polymer, during the charge and discharge process of the battery 10, it is beneficial to further alleviate the internal stress generated by the volume change of the core 11212, thereby further reducing the risk of expansion and rupture of the core 11212, and further reducing the risk of damage to the conductive network of the negative electrode. In addition, the problem of large stress accumulation at the negative electrode polar material layer 112 due to the volume change of the inner core 11212 can be further prevented, thereby further avoiding the rupture of the negative electrode polar material layer 112, and further avoiding the loss of electrical contact between silicon-based material particles and between silicon-based material particles and the negative electrode current collector 111, and the problem of partial detachment of the negative electrode polar material layer 112 from the negative electrode current collector 111, which is conducive to further improving the capacity and service life of the battery 10. The hydrogen bond type supramolecular polymer has good bonding performance, which is conducive to further improving the bonding strength between two adjacent active material particles 1121 in the negative electrode polar material layer 112 and between the active material particles 1121 and the conductive additive, improving the structural strength of the negative electrode polar material layer 112, and also conducive to further improving the bonding strength between the negative electrode polar material layer 112 and the negative electrode current collector 111, thereby further preventing the partial detachment of the negative electrode polar material layer 112 from the negative electrode current collector 111, resulting in the increase of the internal resistance and capacity loss of the battery 10.

[0119] Of course, it can be understood that in other examples, the supramolecular polymer may also be other types of supramolecular polymers, for example, the aforementioned complex-type supramolecular polymer or π-π-type supramolecular polymer.

[0120] In some embodiments, the flexible coating layer 11211 can be directly formed of a supramolecular polymer, so that the material composition is simple, the production is convenient, the cost is reduced, and the elastic deformation ability and bonding performance of the flexible coating layer 11211 are improved.

[0121] Of course, it is understood that in other examples, the flexible coating layer 11211 may also include a conductive material. For example, the flexible coating layer 11211 is formed by mixing a supramolecular polymer and a conductive material. In this way, the flexible coating layer 11211 can be used to conduct electricity, so that a conductive network is formed between the core 11212 and the conductive additive 1122, thereby improving the charge and discharge efficiency of the battery 10.

[0122] Exemplarily, the conductive material includes one or two or more of conductive carbon black, graphene, carbon nanotubes, and graphite.

[0123] In some embodiments, the negative electrode polar material layer 112 is composed of a conductive additive 1122 and active material particles 1121. That is, the negative electrode polar material layer 112 only includes the conductive additive 1122 and the active material particles 1121, and no longer includes a binder, thereby reducing material costs.

[0124] In some embodiments, the conductive additive 1122 may include additives in two forms of granular additives, linear additives, and flake additives. For example, the conductive additive 1122 includes a granular additive and a linear additive. In another example, the conductive additive 1122 includes a granular additive and a flake additive. In another example, the conductive additive 1122 includes a linear additive and a flake additive. In other examples, the conductive additive 1122 may include additives in three forms of granular additives, linear additives, and flake additives. It is sufficient to ensure that the conductive additive 1122 includes additives in at least two forms of granular additives, linear additives, and flake additives.

[0125] In this way, conductive additives 1122 of different forms can complement each other, increase the contact area between conductive additives 1122, and improve the distribution density of conductive additives 1122 in the negative electrode polar material layer 112, so that conductive additives 1122 of different forms can be used to construct a conductive network in the negative electrode polar material layer 112 to form a conductive path. In addition, conductive additives 1122 of different forms complement each other to increase the contact area, which is conducive to ensuring the conductivity of the negative electrode polar material layer 112 under the premise of a lower amount of conductive additives 1122. In addition, conductive additives 1122 of different forms have different degrees of mutual interlocking with the flexible coating layer 11211. The use of conductive additives 1122 of different forms is conducive to compensating for the problem that a single form of conductive additive 1122 cannot form a conductive path with the core 11212 due to its weak interlocking ability with the flexible coating layer 11211, and is more conducive to the construction of a conductive path between the core 11212 in the active material particle 1121 and the conductive additive 1122.

[0126] It is worth noting that, in the present application, a linear additive refers to an additive extending in a linear shape, for example, an additive in a one-dimensional form, and the linear shape includes but is not limited to a straight line, a curve or a broken line. A sheet-like additive refers to an additive that is particularly thin in a certain dimension and forms a thin sheet, for example, an additive in a two-dimensional form. A granular additive refers to an additive that is spherical or irregular, and its size in each direction does not differ too much, for example, a three-dimensional additive. In addition, in other examples, the conductive additive 1122 can also be in the form of a granular additive, a linear additive, and a sheet-like additive.

[0127] In some specific examples, the linear additive includes carbon nanotubes and / or carbon fibers. That is, the linear additive may be carbon nanotubes, carbon fibers, or both.

[0128] Carbon nanotubes can be divided into single-walled carbon nanotubes and multi-walled carbon nanotubes. One-dimensional carbon nanotubes are similar to fibers and are long and cylindrical, with a hollow interior. Carbon nanotubes have good mechanical properties. Specifically, carbon nanotubes have high elastic modulus and high strength, and the structure of carbon nanotubes is highly stable. Using carbon nanotubes as conductive additives 1122 can better form a complete conductive network, which is in point-line contact with active material particles 1121, which is beneficial to improving the conductivity of the negative electrode plate 11 and increasing the capacity of the battery 10.

[0129] Carbon fiber is a high-strength and high-elastic modulus fiber material with a carbon content of more than 90%. In addition to having good mechanical properties, carbon fiber also has good high temperature resistance and friction resistance, and the weight of carbon fiber is very light. Using carbon fiber as a conductive additive 1122 can easily form a good conductive network and show good conductivity, thereby reducing electrode polarization, reducing the internal resistance of the battery 10 and improving the performance of the battery 10. The carbon fiber is also in point-line contact with the active material particles 1121, which is beneficial to improve the conductivity of the negative electrode plate 11 and increase the capacity of the battery 10.

[0130] In some embodiments, the flake additive includes flake graphene and / or flake graphite. Exemplarily, the flake graphene can be single-layer graphene, double-layer graphene or few-layer graphene.

[0131] Among them, single-layer graphene refers to a two-dimensional carbon material composed of a layer of carbon atoms periodically and closely stacked in a benzene ring structure (i.e., a hexagonal honeycomb structure).

[0132] Double-layer graphene refers to a two-dimensional carbon material composed of two layers of carbon atoms that are periodically and closely stacked in a benzene ring structure (i.e., a hexagonal honeycomb structure) in different stacking ways (including AB stacking, AA stacking, etc.).

[0133] Few-layer graphene refers to a two-dimensional carbon material composed of 3-10 layers of carbon atoms periodically and tightly stacked in a benzene ring structure (i.e., a hexagonal honeycomb structure) in different stacking methods (including ABC stacking, ABA stacking, etc.).

[0134] Graphene has high structural strength and good toughness. Due to its unique sheet structure (two-dimensional structure), the contact with the active material particles 1121 is point-to-surface contact, which can maximize the use of the conductive additive 1122, easily form a good conductive network, and show good conductivity. Under the premise of reducing the amount of conductive additive 1122, more active material particles 1121 can be used to increase the capacity of the battery 10.

[0135] Similarly, flake graphite can be a single layer or 2-10 layers.

[0136] The flake graphite also has good electrical conductivity. The flake graphite and the active material particles 1121 are in point-to-surface contact, which can form a conductive network structure of a certain scale and improve the conductive efficiency.

[0137] In some embodiments, the granular additive includes carbon black and / or graphite. The high specific surface area and compact packing of carbon black particles are conducive to close contact between particles, forming a good conductive network, which is conducive to improving conductivity.

[0138] Graphite also has good electrical conductivity. The graphite particles and the active material particles 1121 are in point contact, which can form a conductive network structure of a certain scale and improve the conductive efficiency.

[0139] In some embodiments, the peel strength of the flexible coating layer 11211 has a value range greater than or equal to 10 N / m. That is, in the negative electrode plate 11, when the flexible coating layer 11211 is peeled off from the core 11212, the required peel strength has a value range greater than or equal to 10 N / m. As a result, the bonding strength between the flexible coating layer 11211 and the core 11212 is high, which is beneficial to improve the bonding strength between the active material particles 1121 and between the active material particles 1121 and the negative electrode current collector 111, thereby effectively preventing part of the negative electrode polar material layer 112 from peeling off from the negative electrode current collector 111 and entering the electrolyte 3 during the charge and discharge process of the battery 10. Furthermore, it can avoid the problem of loss of electrical contact between silicon-based material particles and between silicon-based material particles and negative electrode current collector 111 due to cracking and peeling of part of the negative electrode polar material layer 112, or even part of the negative electrode polar material layer 112 falling off from the negative electrode current collector 111, which causes increased internal resistance and capacity loss of the battery 10, which is beneficial to improving the capacity of the battery 10.

[0140] Exemplarily, the peel strength of the flexible coating layer 11211 has a value range of less than or equal to 20 N / m. This makes it easier to select a suitable material to manufacture the flexible coating layer 11211. For example, the peel strength of the flexible coating layer 11211 has a value of 11 N / m, 12 N / m, 13 N / m, 14 N / m, or 15 N / m.

[0141] It is worth noting that when testing the peel strength of the flexible coating layer 11211, the active material particles 1121 can be first separated from the negative electrode polar material layer 112. Then, a peel strength tester (also known as a composite strength tester, a 180 degree peel strength tester, a peel tester, or an electronic peel tester) is used for testing.

[0142] In some embodiments, the elastic modulus of the flexible coating layer 11211 is in the range of 0.3 GPa to 8 GPa, which is helpful to ensure the elastic deformation capability of the flexible coating layer 11211 .

[0143] Exemplarily, the elastic modulus of the flexible coating layer 11211 is 0.5 GPa, 0.6 GPa, 0.8 GPa, 0.9 GPa, 1 GPa, 1.2 GPa, 1.5 GPa, 1.7 GPa, 1.8 GPa, 2 GPa, 2.1 GPa, 2.5 GPa, 2.8 GPa, 3 GPa, 3.2 GPa, 3.5 GPa, 3.8 GPa, 4 GPa, 4.2 GPa, 4.5 GPa, 4.8 GPa, 5 GPa, 5.2 GPa, 5.5 GPa, 5.8 GPa, 6 GPa, 6.2 GPa, 6.5 GPa, 6.7 GPa, 7 GPa, 7.2 GPa, 7.5 GPa, or 7.8 GPa. This is conducive to ensuring the elastic deformation capacity of the flexible coating layer 11211.

[0144] In some embodiments, the material forming the supramolecular polymer includes a first material and a second material.

[0145] Wherein, the first material includes a polymeric acid and / or a polymeric anhydride. Exemplarily, the first material is a polymeric acid or a polymeric anhydride. Exemplarily, the first material is a combination of a polymeric acid and a polymeric anhydride. Wherein, the polymeric anhydride is formed by dehydrating the polymeric acid.

[0146] Exemplarily, the polyacid includes one or more of monomeric fatty acids, dimerized fatty acids, and trimerized fatty acids. Exemplarily, the polyacid is a monomeric fatty acid, a dimerized fatty acid, or a trimerized fatty acid. Exemplarily again, the polyacid includes two of monomeric fatty acids, dimerized fatty acids, and trimerized fatty acids, for example, the polyacid includes a monomeric fatty acid and a dimerized fatty acid. For another example, the polyacid includes a monomeric fatty acid and a trimerized fatty acid. For another example, the polyacid includes a dimerized fatty acid and a trimerized fatty acid. For another example, the polyacid includes a monomeric fatty acid, a dimerized fatty acid, and a trimerized fatty acid. Exemplarily again, the polyacid includes a monomeric fatty acid, a dimerized fatty acid, and a trimerized fatty acid.

[0147] The second material includes polyol and / or polyamine. Exemplarily, the second material is polyol or polyamine. Exemplarily, the second material is a combination of polyol and polyamine.

[0148] Exemplarily, the polyamine includes but is not limited to at least one of diethylenetriamine, triethylenetetramine, ethylenediamine, propylenetriamine, etc. Exemplarily, the polyamine includes diethylenetriamine, triethylenetetramine, ethylenediamine or propylenetriamine. Exemplarily again, the polyamine includes diethylenetriamine and triethylenetetramine. Exemplarily again, the polyamine includes diethylenetriamine and ethylenediamine. Exemplarily again, the polyamine includes triethylenetetramine and ethylenediamine. Exemplarily again, the polyamine includes diethylenetriamine, triethylenetetramine and ethylenediamine. Exemplarily again, the polyamine includes diethylenetriamine, triethylenetetramine and ethylenediamine. Exemplarily again, the polyamine includes diethylenetriamine, triethylenetetramine and ethylenediamine.

[0149] Exemplarily, the polyol includes ethylene glycol and / or glycerol.

[0150] The supramolecular polymer formed by the first material and the second material has good elastic deformation ability and bonding performance, and the material is cheap and low in cost.

[0151] In some embodiments, when the weight of the second material is 1 part, the weight of the first material ranges from 2 parts to 10 parts. In this way, the ratio of the first material to the second material is reasonable, which is conducive to obtaining a supramolecular polymer with excellent elastic deformation ability and bonding performance.

[0152] Parts by weight represent the mass ratio of several substances. Here, 1 part is 1g, for example, the mass of the second material is 1g, and the mass of the first material is 2g to 10g. In other words, when the mass of the second material is 1g, the mass of the first material is any value between 2g and 10g.

[0153] In some embodiments, when the weight of the second material is 1 part, the weight of the first material ranges from 4 parts to 8 parts. In this way, the ratio of the first material to the second material is more reasonable, which is conducive to obtaining a supramolecular polymer with excellent elastic deformation ability and bonding performance.

[0154] Exemplarily, when the weight portion of the second material is 1 part, the weight portion of the first material is 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts or 7.5 parts.

[0155] In some embodiments, the ratio of the equivalent diameter of the active material particles 1121 to the equivalent diameter of the core 11212 is greater than 1 and less than or equal to 1.3. Thus, by limiting the ratio of the equivalent diameter of the active material particles 1121 to the equivalent diameter of the core 11212 to be greater than 1 and less than or equal to 1.3, it is helpful to limit the thickness of the flexible coating layer 11211 within a reasonable range, which is helpful to ensure the elastic deformation ability and bonding performance of the flexible coating layer 11211 on the one hand, and to ensure the structural strength of the flexible coating layer 11211 on the other hand.

[0156] Illustratively, the ratio of the equivalent diameter of the active material particle 1121 to the equivalent diameter of the inner core 11212 is 1.1, 1.15, 1.18, 1.2, 1.21, 1.23, 1.25, 1.26, 1.28, or 1.29.

[0157] The equivalent diameter refers to the equivalent spherical diameter (ESD), which refers to the diameter of a sphere with the same volume as an irregular-shaped object. The equivalent diameter of the active material particle 1121 is the diameter of a sphere with the same volume as the outer surface of the active material particle 1121. When the active material particle 1121 is spherical, the equivalent diameter is the outer diameter of the active material particle 1121. Similarly, the equivalent diameter of the inner core 11212 is the diameter of a sphere with the same volume as the outer surface of the inner core 11212. When the inner core 11212 is spherical, the equivalent diameter is the outer diameter of the inner core 11212.

[0158] In some examples, the equivalent diameter of the core 11212 is nanometer-scale, that is, the equivalent diameter of the core 11212 is greater than or equal to 1 nanometer (nm) and less than 1000nm. Specifically, the equivalent of the core 11212 can be 5nm, 10nm, 20nm, 100nm, 200nm, 500nm, 800nm, 900nm or 950nm. In this way, compared with the core 11212 of a large size, it is beneficial to reduce the volume effect of the core 11212 during the charge and discharge process of the battery 10, facilitate the uniform distribution of more active material particles 1121 in the negative electrode polar material layer 112, and improve the charge and discharge efficiency of the battery 10.

[0159] In some other examples, the equivalent diameter of the core 11212 is in the micrometer level. That is, the equivalent diameter of the core 11212 is greater than or equal to 1 micrometer (um) and less than 1000um. Specifically, the equivalent diameter of the core 11212 can be 5um, 10um, 20um, 100um, 200um, 500um, 800um, 900um or 950um. In this way, it is more conducive to forming a flexible coating layer 11211 on the core 11212, and improving the bonding strength between the flexible coating layer 11211 and the core 11212.

[0160] In some embodiments, the equivalent diameter of the core 11212 ranges from 10 nm to 30 um, that is, 10 nm to 30000 nm. In this way, on the one hand, it is helpful to prevent the problem that the equivalent diameter of the core 11212 is set too small, which is not conducive to forming the flexible coating layer 11211 on the surface of the core 11212, and the bonding strength between the flexible coating layer 11211 and the core 11212 is weak. On the other hand, it is helpful to prevent the problem that the volume change of the core 11212 during the charge and discharge process is too large due to setting the size of the core 11212 too large. That is, the equivalent diameter of the inner core 11212 ranges from 10 nm to 30 um, which makes the size design of the inner core 11212 more reasonable, which can not only ensure the connection strength between the flexible coating layer 11211 and the inner core 11212, but also reduce the volume change of the inner core 11212 during the charging and discharging process of the battery 10, and facilitate the uniform distribution of more active material particles 1121 in the negative electrode polar material layer 112, thereby improving the charging and discharging efficiency of the battery 10.

[0161] Exemplarily, the equivalent diameter of the core 11212 ranges from 80 nm to 25 um. Further, the equivalent diameter of the core 11212 ranges from 150 nm to 10 um.

[0162] The present application also provides a method for processing the negative electrode sheet 11 in the above embodiment. Figure 8 , Figure 8 This is a flow chart of a method for processing a negative electrode plate 11 provided in an embodiment of the present application. The processing method comprises the following steps:

[0163] S10 : providing a negative electrode polar material layer 112 on the surface of the negative electrode current collector 111 .

[0164] Exemplarily, the negative electrode current collector 111 is made of copper.

[0165] The negative electrode polar material layer 112 includes active material particles 1121 and a conductive additive 1122. The active material particles 1121 include a core 11212 and a flexible coating layer 11211.

[0166] The material of the core 11212 includes silicon-based material particles. Exemplarily, the core 11212 is silicon-based material particles, that is, the core 11212 only includes silicon-based material particles and does not include other materials. Exemplarily, in addition to silicon-based material particles, the core 11212 may also include other materials, such as graphite particles.

[0167] Specifically, the silicon-based material particles include at least one of silicon particles, silicon dioxide particles, silicon monoxide particles, and silicon-carbon composite material particles. That is, the silicon-based material particles include one or more of silicon particles, silicon dioxide particles, silicon monoxide particles, and silicon-carbon composite material particles.

[0168] Exemplarily, the silicon-based material particles are silicon particles, silicon dioxide particles, silicon monoxide particles, or silicon-carbon composite material particles.

[0169] In another exemplary embodiment, the silicon-based material particles include two or more of silicon particles, silicon dioxide particles, silicon monoxide particles and silicon-carbon composite material particles. For example, the silicon-based material particles include silicon particles and silicon dioxide particles. Alternatively, the silicon-based material particles include silicon particles and silicon monoxide particles. Alternatively, the silicon-based material particles include silicon particles and silicon-carbon composite material particles. Alternatively, the silicon-based material particles include silicon particles, silicon dioxide particles and silicon monoxide particles. Alternatively, the silicon-based material particles include silicon particles, silicon dioxide particles and silicon-carbon composite material particles. Alternatively, the silicon-based material particles include silicon particles, silicon dioxide particles, silicon monoxide particles and silicon-carbon composite material particles. Alternatively, the silicon-based material particles include silicon particles, silicon dioxide particles, silicon monoxide particles and silicon-carbon composite material particles.

[0170] The flexible coating layer 11211 wraps the inner core 11212. For example, the flexible coating layer 11211 adheres to and wraps the outer surface of the inner core 11212, so that the structure is simple and easy to process and manufacture. In another exemplary embodiment, the flexible coating layer 11211 wraps the inner core 11212, and one or more flexible wrapping layers wrapping the inner core 11212 can be further arranged between the flexible coating layer 11211 and the inner core 11212.

[0171] The material of the flexible coating layer 11211 includes supramolecular polymers. Since supramolecular polymers are a type of polymer connected by non-covalent bonds. The interaction of non-covalent bonds is reversible, that is, the non-covalent bonds in the supramolecular polymers can continuously break and generate. Therefore, the supramolecular polymer can respond to certain external stimuli, withdraw the stimulus, and restore the initial state. During the charging and discharging process, when the volume of the silicon-based material particles increases, the non-covalent bonds J in the supramolecular polymers continuously break and regenerate, so that the flexible coating layer 11211 can adapt to the volume changes of the silicon-based material particles and continuously produce tensile deformation. When the volume of the silicon-based material particles decreases, the non-covalent bonds J in the supramolecular polymers continuously break and regenerate, so that the flexible coating layer 11211 can adapt to the volume changes of the silicon-based material particles and continuously produce shrinkage deformation. Therefore, the flexible coating layer 11211 has excellent elastic deformation ability. In addition, the supramolecular polymer also has certain adhesive properties, thus enabling the flexible covering layer 11211 to have certain adhesive capabilities.

[0172] In this way, during the charge and discharge process of the battery 10, the flexible coating layer 11211 can have a certain restraining effect on the volume expansion of the core 11212, and to a certain extent alleviate the internal stress caused by the volume change of the core 11212, thereby reducing the risk of expansion and rupture of the core 11212 to a certain extent, and further reducing the risk of damage to the conductive network of the negative electrode. In addition, the flexible coating layer 11211 can also play a role in isolating the core 11212 and the electrolyte 3, thereby avoiding the problem of regeneration due to the rupture of the SEI film, avoiding the consumption of lithium ions, and being beneficial to improving the capacity and service life of the battery. In addition, it can also prevent the problem of large stress accumulation at the negative electrode polar material layer 112 caused by the volume change of the core 11212 to a certain extent, thereby avoiding the rupture of the negative electrode polar material layer 112, and further avoiding the loss of electrical contact between the silicon-based material particles and between the silicon-based material particles and the negative electrode current collector 111, and the problem of part of the negative electrode polar material layer 112 falling off from the negative electrode current collector 111, which is beneficial to improving the capacity and service life of the battery 10. In addition, since the supramolecular polymer has certain adhesive properties, in the negative electrode polar material layer 112, the two adjacent active material particles 1121 and the active material particles 1121 and the conductive additive are conducive to bonding with the help of the flexible coating layer 11211, thereby improving the structural strength of the negative electrode polar material layer 112, and it is also beneficial to improve the bonding strength between the negative electrode polar material layer 112 and the negative electrode current collector 111, thereby further preventing part of the negative electrode polar material layer 112 from falling off the negative electrode current collector 111, causing the internal resistance of the battery 10 to increase and the capacity loss to be caused. It is also beneficial to use supramolecular polymers to replace the adhesive in the above embodiment, thereby eliminating the setting of the adhesive and reducing material costs.

[0173] It should be noted that step S10 may specifically include: disposing a negative electrode polar material layer 112 on one side surface of the negative electrode current collector 111 in the thickness direction, so that the negative electrode polar material layer 112 is in contact with the single side surface of the negative electrode current collector 111. Step S10 may also specifically include: disposing a negative electrode polar material layer 112 on both side surfaces of the negative electrode current collector 111 in the thickness direction, so that the negative electrode polar material layer 112 is in contact with the single side surface of the negative electrode current collector 111.

[0174] In some embodiments, see Fig. 9 , Fig. 9 Based on Figure 8 A specific flow chart of step S10 in the method for processing the negative electrode plate 11 shown in FIG. In this embodiment, step S10 specifically includes the following steps:

[0175] Step S11: In a protective gas atmosphere, heating the first material and the second material so that the first material and the second material react to obtain a supramolecular polymer slurry.

[0176] The protective gas may be nitrogen or an inert gas, which may include but is not limited to argon and helium.

[0177] In some embodiments, the first material includes a polymeric acid and / or a polymeric anhydride. Exemplarily, the first material is a polymeric acid or a polymeric anhydride. Exemplarily, the first material is a combination of a polymeric acid and a polymeric anhydride. The polymeric anhydride is formed by dehydrating the polymeric acid.

[0178] Exemplarily, the polyacid includes one or more of monomeric fatty acids, dimerized fatty acids, and trimerized fatty acids. Exemplarily, the polyacid is a monomeric fatty acid, a dimerized fatty acid, or a trimerized fatty acid. Exemplarily again, the polyacid includes two of monomeric fatty acids, dimerized fatty acids, and trimerized fatty acids, for example, the polyacid includes a monomeric fatty acid and a dimerized fatty acid. For another example, the polyacid includes a monomeric fatty acid and a trimerized fatty acid. For another example, the polyacid includes a dimerized fatty acid and a trimerized fatty acid. For another example, the polyacid includes a monomeric fatty acid, a dimerized fatty acid, and a trimerized fatty acid. Exemplarily again, the polyacid includes a monomeric fatty acid, a dimerized fatty acid, and a trimerized fatty acid.

[0179] The second material includes polyol and / or polyamine. Exemplarily, the second material is polyol or polyamine. Exemplarily, the second material is a combination of polyol and polyamine.

[0180] Exemplarily, the polyamine includes but is not limited to at least one of diethylenetriamine, triethylenetetramine, ethylenediamine, propylenetriamine, etc. Exemplarily, the polyamine includes diethylenetriamine, triethylenetetramine, ethylenediamine or propylenetriamine. Exemplarily again, the polyamine includes diethylenetriamine and triethylenetetramine. Exemplarily again, the polyamine includes diethylenetriamine and ethylenediamine. Exemplarily again, the polyamine includes triethylenetetramine and ethylenediamine. Exemplarily again, the polyamine includes diethylenetriamine, triethylenetetramine and ethylenediamine. Exemplarily again, the polyamine includes diethylenetriamine, triethylenetetramine and ethylenediamine. Exemplarily again, the polyamine includes diethylenetriamine, triethylenetetramine and ethylenediamine.

[0181] Exemplarily, the polyol includes ethylene glycol and / or glycerol.

[0182] The supramolecular polymer formed by the first material and the second material has good elastic deformation ability and bonding performance, and the material is cheap and low in cost.

[0183] In some embodiments, when the weight of the second material is 1 part, the weight of the first material ranges from 2 parts to 10 parts. In this way, the ratio of the first material to the second material is reasonable, which is conducive to obtaining a supramolecular polymer with excellent elastic deformation ability and bonding performance.

[0184] Specifically, when the weight of the second material is 1 part, the weight of the first material ranges from 4 parts to 8 parts. This is conducive to obtaining a supramolecular polymer with excellent elastic deformation ability and adhesive properties.

[0185] Specifically, step S11 may include: in a protective gas atmosphere, using a stirrer to fully mix and react the first material and the second material to obtain a supramolecular polymer slurry. In this way, the mixing uniformity can be improved. The stirrer includes but is not limited to a propeller stirrer, a turbine stirrer, a paddle stirrer, an anchor stirrer, a ribbon stirrer, a magnetic stirrer, a magnetic heating stirrer, a folding blade stirrer, a variable frequency double-layer stirrer, and a side-entry stirrer.

[0186] Step S12: placing a supramolecular polymer slurry on the surface of the inner core 11212 to form active material particles 1121 having a flexible coating layer 11211;

[0187] Specifically, in step S12 , the supramolecular polymer slurry is coated on the outer surface of the inner core 11212 to form active material particles 1121 having a flexible coating layer 11211 .

[0188] In this way, the flexible coating layer 11211 is formed of only supramolecular polymer, that is, the flexible coating layer 11211 is formed of a single supramolecular polymer material. In this way, the material composition is simple, easy to manufacture, and conducive to reducing costs, and is conducive to improving the elastic deformation ability and bonding performance of the flexible coating layer 11211.

[0189] In some embodiments, the peel strength of the flexible coating layer 11211 has a value range greater than or equal to 10 N / m. That is, when the flexible coating layer 11211 is peeled off from the core 11212, the required peel strength has a value range greater than or equal to 10 N / m. As a result, the bonding strength between the flexible coating layer 11211 and the core 11212 is high, which is beneficial to improve the bonding strength between the active material particles 1121 and between the active material particles 1121 and the negative electrode current collector 111, thereby effectively preventing part of the negative electrode polar material layer 112 from peeling off from the negative electrode current collector 111 and entering the electrolyte 3 during the charge and discharge process of the battery 10. Furthermore, it can avoid the problem of loss of electrical contact between silicon-based material particles and between silicon-based material particles and negative electrode current collector 111 due to cracking and peeling of part of the negative electrode polar material layer 112, or even part of the negative electrode polar material layer 112 falling off from the negative electrode current collector 111, which causes increased internal resistance and capacity loss of the battery 10, which is beneficial to improving the capacity of the battery 10.

[0190] Exemplarily, the peel strength of the flexible coating layer 11211 has a value range of less than or equal to 20 N / m. This makes it easier to select a suitable material to manufacture the flexible coating layer 11211. For example, the peel strength of the flexible coating layer 11211 has a value of 11 N / m, 12 N / m, 13 N / m, 14 N / m, or 15 N / m.

[0191] In some embodiments, the elastic modulus of the flexible coating layer 11211 is in the range of 0.3 GPa to 8 GPa, which is helpful to ensure the elastic deformation capability of the flexible coating layer 11211 .

[0192] Exemplarily, the elastic modulus of the flexible coating layer 11211 is 0.5 GPa, 0.6 GPa, 0.8 GPa, 0.9 GPa, 1 GPa, 1.2 GPa, 1.5 GPa, 1.7 GPa, 1.8 GPa, 2 GPa, 2.1 GPa, 2.5 GPa, 2.8 GPa, 3 GPa, 3.2 GPa, 3.5 GPa, 3.8 GPa, 4 GPa, 4.2 GPa, 4.5 GPa, 4.8 GPa, 5 GPa, 5.2 GPa, 5.5 GPa, 5.8 GPa, 6 GPa, 6.2 GPa, 6.5 GPa, 6.7 GPa, 7 GPa, 7.2 GPa, 7.5 GPa, or 7.8 GPa. This is conducive to ensuring the elastic deformation capacity of the flexible coating layer 11211.

[0193] Step S13: fully mixing the active material particles 1121 and the conductive additive 1122 to obtain a polar slurry;

[0194] Specifically, step S13 may include: using a mixer to fully mix the active material particles 1121 and the conductive additive 1122 to obtain a polar slurry, so that the mixing uniformity can be improved.

[0195] Step S14: placing the polar slurry on the surface of the negative electrode current collector 111 to obtain the negative electrode polar material layer 112.

[0196] Specifically, step S14 may include: coating the polar slurry on the surface of the negative electrode current collector 111 to obtain the negative electrode polar material layer 112 .

[0197] In this way, the negative electrode polar material layer 112 is formed by the conductive additive 1122 and the active material particles 1121, which saves the setting of the binder and is conducive to reducing the material cost. In addition, the negative electrode polar material layer 112 can be closely attached to the negative electrode current collector 111, which can improve the bonding strength between the negative electrode polar material layer 112 and the negative electrode current collector 111. This method is simple, the conditions are easy to control, and it is suitable for industrial production.

[0198] In some embodiments, the conductive additive 1122 may include additives in two forms of granular additives, linear additives, and flake additives. For example, the conductive additive 1122 includes a granular additive and a linear additive. For another example, the conductive additive 1122 includes a granular additive and a flake additive. For another example, the conductive additive 1122 includes a linear additive and a flake additive. In other examples, the conductive additive 1122 may include additives in three forms of granular additives, linear additives, and flake additives.

[0199] In this way, conductive additives 1122 of different forms can complement each other, increase the contact area between conductive additives 1122, and improve the distribution density of conductive additives 1122 in the negative electrode polar material layer 112, so that conductive additives 1122 of different forms can be used to construct a conductive network in the negative electrode polar material layer 112 to form a conductive path. In addition, conductive additives 1122 of different forms complement each other to increase the contact area, which is conducive to ensuring the conductivity of the negative electrode polar material layer 112 under the premise of a lower amount of conductive additives 1122. In addition, conductive additives 1122 of different forms have different degrees of mutual interlocking with the flexible coating layer 11211. The use of conductive additives 1122 of different forms is conducive to compensating for the problem that a single form of conductive additive 1122 cannot form a conductive path with the core 11212 due to its weak interlocking ability with the flexible coating layer 11211, and is more conducive to the construction of a conductive path between the core 11212 in the active material particle 1121 and the conductive additive 1122.

[0200] Of course, it can be understood that in other examples, the conductive additive 1122 can be in the form of a granular additive, a linear additive, or a flake additive.

[0201] In some specific examples, the linear additive includes carbon nanotubes and / or carbon fibers. That is, the linear additive may be carbon nanotubes, carbon fibers, or both.

[0202] Carbon nanotubes can be divided into single-walled carbon nanotubes and multi-walled carbon nanotubes. One-dimensional carbon nanotubes are similar to fibers and are long and cylindrical, with a hollow interior. Carbon nanotubes have good mechanical properties. Specifically, carbon nanotubes have high elastic modulus and high strength, and the structure of carbon nanotubes is highly stable. Using carbon nanotubes as conductive additives 1122 can better form a complete conductive network, which is in point-line contact with active material particles 1121, which is beneficial to improving the conductivity of the negative electrode plate 11 and increasing the capacity of the battery 10.

[0203] Carbon fiber is a high-strength and high-elastic modulus fiber material with a carbon content of more than 90%. In addition to having good mechanical properties, carbon fiber also has good high temperature resistance and friction resistance, and the weight of carbon fiber is very light. Using carbon fiber as a conductive additive 1122 can easily form a good conductive network and show good conductivity, thereby reducing electrode polarization, reducing the internal resistance of the battery 10 and improving the performance of the battery 10. The carbon fiber is also in point-line contact with the active material particles 1121, which is beneficial to improve the conductivity of the negative electrode plate 11 and increase the capacity of the battery 10.

[0204] In some embodiments, the flake additive includes flake graphene and / or flake graphite. Graphene has high structural strength and good toughness. And due to its unique flake structure (two-dimensional structure), the contact with the active material particles 1121 is point-to-surface contact, which can maximize the use of the conductive additive 1122, easily form a good conductive network, and show good conductivity. Under the premise of reducing the amount of the conductive additive 1122, more active material particles 1121 can be used to increase the capacity of the battery 10.

[0205] The flake graphite also has good electrical conductivity. The flake graphite and the active material particles 1121 are in point-to-surface contact, which can form a conductive network structure of a certain scale and improve the conductive efficiency.

[0206] In some embodiments, the granular additive includes carbon black and / or graphite. The high specific surface area and compact packing of carbon black particles are conducive to close contact between particles, forming a good conductive network, which is conducive to improving conductivity.

[0207] Graphite also has good electrical conductivity. The graphite particles and the active material particles 1121 are in point contact, which can form a conductive network structure of a certain scale and improve the conductive efficiency.

[0208] See also Fig.10 , Fig.10 Based on Fig. 9 The specific flow chart of step S12 in the processing method of the negative electrode plate 11 is shown. In this embodiment, step S12 specifically includes the following steps:

[0209] Step S121: disposing supramolecular polymer slurry on the surface of the inner core 11212 to cover the surface of the inner core 11212 with the supramolecular polymer slurry;

[0210] Step S122: heating the supramolecular polymer slurry on the surface of the inner core 11212 at a second preset temperature for a second preset time;

[0211] Specifically, the second preset temperature ranges from 70° C. to 120° C. Exemplarily, the second preset temperature ranges from 90° C. to 110° C. For example, the second preset temperature is 91° C., 92° C., 93° C., 94° C., 95° C., 96° C., 97° C., 98° C., 99° C., 100° C., 101° C., 102° C., 103° C., 104° C., 105° C., 106° C., 107° C., 108° C., or 109° C.

[0212] Specifically, the value range of the second preset time is 3 minutes to 100 minutes. Exemplarily, the value range of the second preset time is 3 minutes to 10 minutes. For example, the value of the second preset time is 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes or 9 minutes.

[0213] Step S123 : Cooling the supramolecular polymer slurry on the surface of the inner core 11212 to form a flexible coating layer 11211 .

[0214] Since the inner core 11212 includes silicon-based material particles, the surface of the silicon-based material particles has silicon-oxygen bonds, heating the supramolecular polymer slurry on the surface of the inner core 11212 is beneficial to improving the fluidity and diffusivity of the supramolecular polymer slurry, thereby improving the wetting effect between the supramolecular polymer slurry and the surface of the inner core 11212, and on the other hand, it is beneficial for the non-covalent bonds in the supramolecular polymer to bond with the silicon-oxygen bonds after breaking, thereby improving the bonding strength between the flexible coating layer 11211 and the inner core 11212 through these two aspects.

[0215] For some examples, see Fig.11 , Fig.11 Based on Fig.10 The specific flow chart of step S121 in the processing method of the negative electrode plate 11 is shown. In this embodiment, step S121 may include:

[0216] Step S1211: at a third preset temperature, disposing the supramolecular polymer slurry on the surface of the core 11212 to cover the surface of the core 11212 with the supramolecular polymer slurry; wherein the third preset temperature is greater than the room temperature and less than the second preset temperature.

[0217] Step S1212: Cooling the supramolecular polymer slurry, that is, cooling the supramolecular polymer slurry to room temperature.

[0218] Thus, at the third preset temperature, the supramolecular polymer slurry is disposed on the surface of the core 11212 , which is beneficial to improving the fluidity and diffusivity of the supramolecular polymer slurry, thereby improving the wetting effect between the supramolecular polymer slurry and the surface of the core 11212 , and further improving the bonding strength between the coating layer and the core 11212 .

[0219] Exemplarily, the third preset temperature ranges from 40° C. to 50° C. For example, the third preset temperature is 42° C., 45° C., 48° C., or 49° C.

[0220] See also Fig.12 , Fig.12 Based on Figure 8 Another specific flow chart of step S10 in the method for processing the negative electrode sheet 11 shown in FIG. In this embodiment, step S10 specifically includes the following steps:

[0221] Step S11: In a protective gas atmosphere, heating the first material and the second material so that the first material and the second material react to obtain a supramolecular polymer slurry.

[0222] Step S12: placing the supramolecular polymer slurry on the surface of the inner core 11212 to form active material particles 1121 with a flexible coating layer;

[0223] Specifically, in step S12 , the supramolecular polymer slurry is coated on the surface of the inner core 11212 to form active material particles 1121 having a flexible coating layer.

[0224] In this way, the flexible coating layer 11211 is formed of only supramolecular polymer, that is, the flexible coating layer 11211 is formed of a single supramolecular polymer material. In this way, the material composition is simple, easy to manufacture, and conducive to reducing costs, and is conducive to improving the elastic deformation ability and bonding performance of the flexible coating layer 11211.

[0225] Step S13: Fully mix the active material particles 1121, the conductive additive 1122 and the solvent to obtain a polar slurry.

[0226] In this way, adding a solvent can help improve the uniformity of mixing between materials.

[0227] Specifically, step S13 may include: using a stirrer to fully mix the active material particles 1121, the conductive additive 1122 and the solvent to obtain a polar slurry, so that the mixing uniformity can be improved.

[0228] Step S14: placing the polar slurry on the surface of the negative electrode current collector 111. Specifically, step S14 may include: coating the polar slurry on the surface of the negative electrode current collector 111.

[0229] S15 : drying the polar slurry on the negative electrode current collector 111 to volatilize the solvent in the polar slurry, so as to obtain the negative electrode polar material layer 112 .

[0230] The drying process may be a baking process. The baking temperature may be greater than or equal to 70° C. and less than or equal to 90° C. Specifically, the baking temperature may be 70° C., 72° C., 74° C., 76° C., 78° C., 80° C., 84° C., 86° C., 88° C. or 90° C.

[0231] In this way, the negative electrode polar material layer 112 is formed by the conductive additive 1122 and the active material particles 1121, which saves the setting of the binder and is conducive to reducing the material cost. In addition, the negative electrode polar material layer 112 can be closely attached to the negative electrode current collector 111, which can improve the bonding strength between the negative electrode polar material layer 112 and the negative electrode current collector 111. This method is simple, the conditions are easy to control, and it is suitable for industrial production.

[0232] The solvent includes at least one of water and an organic solvent. That is, the solvent can be water, can be an organic solvent, or can include both water and an organic solvent.

[0233] The organic solvent includes ethanol and / or NMP (N-Methylpyrrolidone).

[0234] In other examples, the organic solvent may also include at least one of benzene, toluene, xylene, pentane, hexane, octane, cyclohexane, cyclohexanone, toluene cyclohexanone, chlorobenzene, dichlorobenzene, dichloromethane, methanol, isopropanol, ethyl ether, propylene oxide, methyl acetate, ethyl acetate, propyl acetate, ethyl propionate, acetone, methyl butyl ketone, methyl isobutyl ketone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, acetonitrile, pyridine and phenol.

[0235] The following describes in detail the processing of the negative electrode sheet 11 in the form of different embodiments.

[0236] Embodiment 1

[0237] Under a protective atmosphere, a polyacid having a mass ratio of 4 to 8:1 and diethylenetriamine are cross-linked at 150° C. to 200° C. for 8 to 24 hours to prepare a supramolecular polymer slurry. The polyacid comprises one or more of a fatty acid monomer, a fatty acid dimer, and a fatty acid trimer. The polyacid and diethylenetriamine undergo a cross-linking reaction, and the structure of the resulting supramolecular polymer slurry is a cross-linked structure, which belongs to a hydrogen-bonded supramolecular polymer. It is understood that the supramolecular polymer slurry is in a semi-cured state.

[0238] In an environment of 40°C to 50°C (i.e., the third preset temperature), the supramolecular polymer slurry is placed on the surface of the core 11212; for example, 5 ul of the slurry is coated on the surface of the core 11212 and spread flat. The core 11212 is made of silicon-carbon composite material particles with an equivalent diameter of 8 um.

[0239] Then cool to room temperature.

[0240] In an environment of 100° C. (ie, the second preset temperature), the core 11212 and the supramolecular polymer slurry on the surface of the core 11212 are heated for 5 minutes (ie, the second preset time).

[0241] The supramolecular polymer slurry is cooled to form active material particles 1121 having a flexible coating layer 11211. The thickness of the flexible coating layer 11211 is in the range of 3 to 5 nm.

[0242] The prepared active material particles 1121, conductive carbon black and single-walled carbon nanotubes are fully mixed to prepare a polar slurry without an additional binder;

[0243] The polar slurry is coated on the surface of the negative electrode current collector 111 to form the negative electrode polar material layer 112 .

[0244] Embodiment 2

[0245] Under a protective atmosphere, a polyacid having a mass ratio of 4 to 8:1 and ethylenediamine are subjected to a linear reaction at 80°C to 160°C for 8 to 24 hours to prepare a supramolecular polymer slurry. The polyacid comprises one or more of a fatty acid monomer, a fatty acid dimer, and a fatty acid trimer. The polyacid and ethylenediamine undergo a linear reaction, and the structure of the resulting supramolecular polymer slurry is a linear structure, which belongs to a hydrogen-bonded supramolecular polymer. It is understood that the supramolecular polymer slurry is in a semi-cured state.

[0246] In an environment of 40°C to 50°C (i.e., the third preset temperature), the supramolecular polymer slurry is placed on the surface of the core 11212; for example, 5 ul of the slurry is coated on the surface of the core 11212 and spread flat. The core 11212 is made of silicon-carbon composite material particles with an equivalent diameter of 8 um.

[0247] Then cool to room temperature.

[0248] In an environment of 100° C., the core 11212 and the supramolecular polymer slurry on the surface of the core 11212 are heated for 5 minutes (ie, the second preset time).

[0249] The supramolecular polymer slurry is cooled to form active material particles 1121 having a flexible coating layer 11211. The thickness of the flexible coating layer 11211 is in the range of 3 to 5 nm.

[0250] The prepared active material particles 1121, conductive carbon black and single-walled carbon nanotubes are fully mixed to prepare a polar slurry without an additional binder;

[0251] The polar slurry is coated on the surface of the negative electrode current collector 111 to form the negative electrode polar material layer 112 .

[0252] Embodiment 3

[0253] Under a protective atmosphere, a polyacid having a mass ratio of 4 to 8:1 and glycerol are cross-linked at 150° C. to 250° C. for 8 to 24 hours to prepare a supramolecular polymer slurry. The polyacid comprises one or more of a fatty acid monomer, a fatty acid dimer, and a fatty acid trimer. The polyacid and glycerol undergo a cross-linking reaction, and the structure of the resulting supramolecular polymer slurry is a cross-linked structure, which belongs to a hydrogen-bonded supramolecular polymer. It is understood that the supramolecular polymer slurry is in a semi-cured state.

[0254] In an environment of 40°C to 50°C (i.e., the third preset temperature), the supramolecular polymer slurry is placed on the surface of the core 11212; for example, 5 ul of the slurry is coated on the surface of the core 11212 and spread flat. The core 11212 is made of silicon-carbon composite material particles with an equivalent diameter of 8 um.

[0255] Then cool to room temperature.

[0256] In an environment of 100° C., the core 11212 and the supramolecular polymer slurry on the surface of the core 11212 are heated for 5 minutes (ie, the second preset time).

[0257] The supramolecular polymer slurry is cooled to form active material particles 1121 having a flexible coating layer 11211. The thickness of the flexible coating layer 11211 is in the range of 3 to 5 nm.

[0258] The prepared active material particles 1121, conductive carbon black and single-walled carbon nanotubes are fully mixed to prepare a polar slurry without an additional binder;

[0259] The polar slurry is coated on the surface of the negative electrode current collector 111 to form the negative electrode polar material layer 112 .

[0260] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.

[0261] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A negative electrode sheet, It is characterized in that include: Anode current collector; A negative electrode polar material layer, the negative electrode polar material layer is arranged on the surface of the negative electrode current collector, the negative electrode polar material layer is composed of active material particles and conductive additives; the active material particles include a core and a flexible coating layer, the flexible coating layer wraps the core, the core material includes silicon-based material particles, the flexible coating layer is formed by a supramolecular polymer, the peel strength of the flexible coating layer ranges from greater than or equal to 10N / m; the elastic modulus of the flexible coating layer ranges from 1.2GPa to 8GPa; the ratio of the equivalent diameter of the active material particles to the equivalent diameter of the core is greater than 1 and less than or equal to 1.3; The materials forming the supramolecular polymer include a first material and a second material; the first material includes a polymeric acid and / or a polymeric anhydride, wherein the polymeric anhydride is formed by dehydrating a polymeric acid; wherein the polymeric acid includes one or more of a dimerized fatty acid and a trimerized fatty acid; the second material includes a polyol and / or a polyamine, wherein the polyamine does not include diethylenetriamine; when the weight portion of the second material is 1 part, the weight portion of the first material ranges from 2 parts to 10 parts.

2. The negative electrode sheet according to claim 1, It is characterized in that The flexible covering layer is attached to the outer surface of the inner core.

3. The negative electrode sheet according to claim 1 or 2, It is characterized in that The supramolecular polymer is a hydrogen-bond type supramolecular polymer.

4. The negative electrode sheet according to claim 1, It is characterized in that The conductive additive includes two forms of additives: granular additives and linear additives; or, The conductive additive includes two forms of additives: granular additives and flake additives; or, The conductive additive includes two forms of additives: linear additives and flake additives; or, The conductive additives include additives in three forms: granular additives, linear additives and flake additives.

5. The negative electrode sheet according to claim 4, It is characterized in that The linear additives include carbon nanotubes and / or carbon fibers; The flake additive includes flake graphene and / or flake graphite; The particulate additive includes carbon black and / or graphite.

6. The negative electrode sheet according to any one of claims 1 to 5, It is characterized in that The equivalent diameter of the core ranges from 10 nm to 30 um.

7. A battery, It is characterized in that include: Positive electrode sheet, separator and negative electrode sheet; The negative electrode sheet is the negative electrode sheet according to any one of claims 1 to 6, and the positive electrode sheet and the negative electrode sheet are separated by the separator.

8. An electronic device, It is characterized in that include: Electrical devices; The battery according to claim 7, wherein the battery is electrically connected to the electrical device.

9. A method for processing a negative electrode sheet, It is characterized in that The processing method comprises: A negative electrode polar material layer is arranged on the surface of the negative electrode current collector; wherein the negative electrode polar material layer is composed of active material particles and conductive additives, the active material particles include a core and a flexible coating layer, the flexible coating layer wraps the core, the core includes silicon-based material particles, the flexible coating layer is formed by a supramolecular polymer, the peel strength of the flexible coating layer ranges from greater than or equal to 10N / m; the elastic modulus of the flexible coating layer ranges from 1.2GPa to 8GPa; the ratio of the equivalent diameter of the active material particles to the equivalent diameter of the core is greater than 1 and less than or equal to 1.3; Wherein, a negative electrode polar material layer is arranged on the surface of the negative electrode current collector, including: In a protective gas atmosphere, heating the first material and the second material so that the first material and the second material react to obtain a supramolecular polymer slurry; disposing a supramolecular polymer slurry on the outer surface of the inner core to form active material particles with a flexible coating; thoroughly mixing active material particles and conductive additives to obtain a polar slurry; A polar slurry is disposed on the surface of a negative electrode current collector to obtain a negative electrode polar material layer; wherein the first material comprises a polymeric acid and / or a polymeric anhydride, and the polymeric anhydride is formed by dehydrating a polymeric acid; wherein the polymeric acid comprises one or more of a dimerized fatty acid and a trimerized fatty acid; the second material comprises a polyol and / or a polyamine; when the weight portion of the second material is 1 part, the weight portion of the first material ranges from 2 parts to 10 parts.

10. The method for processing a negative electrode sheet according to claim 9, It is characterized in that A negative electrode polar material layer is arranged on the surface of the negative electrode current collector, comprising: In a protective gas atmosphere, heating the first material and the second material so that the first material and the second material react to obtain a supramolecular polymer slurry; disposing a supramolecular polymer slurry on the surface of the inner core to form active material particles with a flexible coating; mixing active material particles, conductive additives and solvent thoroughly to obtain a polar slurry; Disposing the polar slurry on the surface of the negative electrode current collector; The polar slurry on the negative electrode current collector is dried to volatilize the solvent in the polar slurry to obtain a negative electrode polar material layer.

11. A method for processing a negative electrode sheet according to any one of claims 9 to 10, It is characterized in that The supramolecular polymer slurry is disposed on the surface of the inner core to form active material particles with a flexible coating layer, comprising: Disposing the supramolecular polymer slurry on the surface of the inner core so as to cover the surface of the inner core with the supramolecular polymer slurry; heating the supramolecular polymer slurry on the surface of the inner core for a second preset time at a second preset temperature; The supramolecular polymer slurry is cooled to form a flexible covering layer.

12. The method for processing a negative electrode sheet according to claim 11, It is characterized in that The second preset temperature has a value range of 70° C. to 120° C.; and / or, The second preset time has a value range of 3 minutes to 100 minutes.

13. The method for processing a negative electrode sheet according to claim 11 or 12, It is characterized in that The supramolecular polymer slurry is disposed on the surface of the inner core so as to cover the surface of the inner core with the supramolecular polymer slurry, comprising: At a third preset temperature, the supramolecular polymer slurry is disposed on the surface of the inner core so as to cover the surface of the inner core with the supramolecular polymer slurry; wherein the third preset temperature is greater than room temperature and less than the second preset temperature; The supramolecular polymer slurry is cooled.

14. A method for processing a negative electrode sheet according to any one of claims 9 to 13, It is characterized in that The conductive additive includes two forms of additives: granular additives and linear additives; or, The conductive additive includes two forms of additives: granular additives and flake additives; or, The conductive additive includes two forms of additives: linear additives and flake additives; or, The conductive additives include additives in three forms: granular additives, linear additives and flake additives.