Method for manufacturing terminal protection structure of semiconductor power device

By forming a trench isolation structure between the field limit rings of the fast recovery diode, adjusting the curved surface of the field limit ring, solving the problem of power line concentration caused by the curvature of the field limit ring, improving the reverse breakdown voltage, simplifying the process, and enhancing the Performance of semiconductor power devices.

CN117153863BActive Publication Date: 2024-12-03MINHUAWEI (SHANGHAI) ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311218540.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-20
Publication Date
2024-12-03
Estimated Expiration
2043-09-20

AI Technical Summary

Technical Problem

In the terminal protection structure of the existing fast recovery diode, the junction curvature of the field limit ring leads to concentrated power lines, reducing the reverse breakdown voltage, and the process is complicated.

Method used

By forming a trench isolation structure between the field rings and using the trench isolation structure to adjust the curved surface of the field ring, lowering the curved surface corner angle, preventing power lines from entering the surface of the silicon epitaxial layer, and increasing the reverse breakdown voltage.

Benefits of technology

The reverse breakdown voltage of semiconductor power devices is increased, the manufacturing process is simplified, the electric field rise is reduced, and the reverse characteristics of the device are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117153863B_ABST
    Figure CN117153863B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for manufacturing a terminal protection structure of a semiconductor power device, comprising: step 1, performing ion implantation to form a first implantation region of a main junction. Step 2, performing ion implantation to form a plurality of second implantation regions and forming a field limiting ring of a terminal protection structure; each field limiting ring is formed in a first epitaxial layer outside the first implantation region and has a ring structure, and the radius of the inner edge of each field limiting ring increases from the outer edge of the first implantation region to the outside. Step 3, forming a plurality of first grooves; filling a first dielectric layer in each first groove to form a groove isolation structure. The groove isolation structure is formed between each field limiting ring, between the innermost field limiting ring and the first implantation region, and outside the outermost field limiting ring. Each field limiting ring contacts with the first epitaxial layer to form an auxiliary junction; the contact surface of the auxiliary junction is a first curved surface; the groove isolation structure limits the first curved surface from both sides of the first curved surface. The present invention can improve the reverse breakdown voltage of the terminal protection structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for manufacturing a semiconductor integrated circuit, in particular to a method for manufacturing a terminal protection structure of a semiconductor power device. Background Art

[0002] Fast Recovery Diode (FRD) is a new type of power device that has been introduced in recent years. It is one of the most widely used power semiconductor devices in power electronic equipment. Due to its advantages of good switching performance, short reverse recovery time, reduced forward conduction voltage, large current, high reverse withstand voltage, and small leakage, it is often used in parallel with three-terminal power switching devices (such as IGBT, etc.) in power electronic circuits as high-frequency, high-current freewheeling diodes or rectifiers, and has great development prospects and market demand. From the perspective of withstand voltage range, FRDs less than 1200V are mainly used in variable-frequency home appliances, variable-frequency welding machines, and electric vehicles; FRDs with voltages greater than 1200V-1700V are mainly used in photovoltaic inverters, high-voltage inverters and other industrial products. The continuous development of power electronics technology and consumer electronics technology has opened up a wide range of application fields for semiconductor power devices. With the rapid growth of power electronics technology and consumer electronics, people are increasingly demanding cost reduction.

[0003] For fast recovery diodes, reverse breakdown voltage is one of the most important parameters. It determines the rated power of power electronic devices together with the maximum current capacity. Among them, silicon-based power FRDs usually use a large-area PN junction to ensure high current operation. However, for FRDs working at high voltage, there is inevitably a junction bending effect in the planar process, and the main factors affecting the device breakdown voltage are the electric field concentration caused by the junction bending in the PN junction diffusion window area and the surface electric field concentration caused by the interface charge. Because of these factors, the actual breakdown voltage of the device is only 10% to 30% of the ideal situation. Therefore, in order to ensure that silicon-based FRDs can work normally under high voltage, it is usually necessary to take measures at the outer edge of the device main junction, namely, junction terminal protection technology, such as field plates and field limiting rings, to eliminate the influence of the junction bending effect, weaken the surface electric field strength, and increase the pn junction breakdown voltage of power FRD devices.

[0004] The dielectric of the field plate of the existing fast recovery diode and the dielectric of the field limiting ring isolation are both field oxides located on the surface of the silicon epitaxial layer. However, in the existing fast recovery diode, the terminal field limiting ring, that is, the PN contact surface of the PN junction formed between the P+ injection region and the N- substrate is an approximately elliptical curved surface. The corner portion of the junction curved surface will cause the electric lines to be relatively concentrated and the electric field to rise. At the same time, part of the electric lines will terminate on the surface of the silicon epitaxial layer in the spacing area between the field limiting rings. Both of these situations will cause the reverse breakdown voltage here to be significantly lower than the breakdown voltage of the main junction plane portion, thereby reducing the reverse breakdown voltage of the entire device. If the flatness of the depletion layer during reverse operation can be improved and the termination of the electric lines can be made away from the silicon substrate surface, the breakdown voltage of the terminal portion will be closer to the breakdown voltage of the main junction portion, thereby increasing the breakdown voltage of the entire device and improving the reverse characteristics (breakdown voltage and reverse leakage current) of the fast recovery diode. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for manufacturing a terminal protection structure of a semiconductor power device, which can form a terminal protection structure that adjusts the curved surface of the junction surface of the field limiting ring, thereby reducing the concentration of electric lines caused by the curved surface corners of the junction surface of the field limiting ring, and can also prevent the electric lines from entering the top surface of the epitaxial layer between the field limiting rings, thereby reducing the electric field rise caused thereby, improving the reverse breakdown voltage of the terminal protection structure and further improving the reverse breakdown voltage of the entire semiconductor power device, and can also achieve process simplification.

[0006] In order to solve the above technical problems, the present invention provides a method for manufacturing a terminal protection structure of a semiconductor power device, comprising the following steps:

[0007] Step 1: providing a first epitaxial layer doped with a first conductivity type, and performing second conductivity type ion implantation in a selected region of the first epitaxial layer to form a first implantation region; the first implantation region and the first epitaxial layer form a main junction.

[0008] Step 2: Performing second conductivity type ion implantation in selected areas of the first epitaxial layer to form multiple second implantation regions, each of which forms a field limiting ring; the field limiting ring is a component of a terminal protection structure, and the terminal protection structure surrounds the periphery of the main junction.

[0009] Each of the field limiting rings is formed in the first epitaxial layer outside the first injection region and has a ring structure, and the radius of the inner edge of each of the field limiting rings increases sequentially from the outer edge of the first injection region to the outside.

[0010] Step three: forming a plurality of first trenches in selected regions of the first epitaxial layer; the first trenches are located in a formation region of a terminal protection structure.

[0011] A first dielectric layer is filled in each of the first trenches to form a trench isolation structure.

[0012] The trench isolation structure is formed between the field limiting rings, between the innermost field limiting ring and the first implantation region, and outside the outermost field limiting ring.

[0013] Each of the field limiting rings and the first epitaxial layer contacts to form an auxiliary junction; the contact surface of the auxiliary junction is a first curved surface; the trench isolation structure limits the first curved surface from both sides of the first curved surface to reduce the area of ​​the first curved surface, reduce the corner angles on both sides of the first curved surface, and make the corner positions on both sides of the first curved surface below the top surface of the first epitaxial layer, so as to prevent the concentration of electric lines at the corners on both sides of each of the first curved surfaces and make the electric lines away from the top surface of the first epitaxial layer when the semiconductor power device is reverse biased, thereby improving the reverse breakdown voltage of the terminal protection structure.

[0014] A further improvement is that, before step three, before or after step one or step two, the method further includes:

[0015] A first conductive type heavily doped ion implantation is performed to form a stop ring in the first epitaxial layer outside the outermost field limiting ring.

[0016] A further improvement is that the bottom surface of the first trench is flush with the bottom surface of the field limiting ring, so as to improve the flatness of the depletion layer formed by depletion of each auxiliary junction when the semiconductor power device is reverse biased.

[0017] A further improvement is that the method further comprises the following steps:

[0018] Step 4: forming an interlayer film.

[0019] A top surface of the trench isolation structure is flush with a top surface of the first epitaxial layer, and the interlayer film is formed on the top surfaces of the trench isolation structure and the first epitaxial layer.

[0020] Step 5: forming a contact hole through the interlayer film in a selected area.

[0021] Step six: forming a front metal layer, and patterning the front metal layer to form a front electrode, wherein the front electrode includes a first electrode of the main junction and a terminal field plate.

[0022] The first injection region is connected to the first electrode through the corresponding contact hole at the top.

[0023] Each of the field limiting rings is connected to the corresponding terminal field plate through the corresponding contact hole at the top.

[0024] A further improvement is that in step three, the first dielectric layer is an oxide layer.

[0025] A further improvement is that, in step three, after the growth of the first dielectric layer is completed, the first dielectric layer completely fills the first trench and also extends to the surface of the outer area of ​​the first trench.

[0026] After the growth of the first dielectric layer is completed, the first dielectric layer is planarized to completely remove the first dielectric layer outside the first trench and to make the first dielectric layer in the first trench flush with the top surface of the first trench to form the trench isolation structure.

[0027] A further improvement is that in step three, the first dielectric layer is formed by using the interlayer film.

[0028] In step three, after the first trench is formed, the interlayer film deposition process of step four is directly performed to form a second oxide layer, which completely fills the first trench and extends to the surface of the outer area of ​​the second oxide layer.

[0029] Afterwards, the method further includes planarizing the second oxide layer, and the second oxide layer filled in the first trench after planarization forms the trench isolation structure; and the second oxide layer located on the top of the trench isolation structure and outside the first trench forms the interlayer film.

[0030] A further improvement is that in step three, the first dielectric layer is planarized by chemical mechanical polishing or etching back process.

[0031] A further improvement is that in step four, the second oxide layer is planarized by chemical mechanical polishing or etching back process.

[0032] A further improvement is that there is a distance between the inner edge of the trench isolation structure located between the outer edge of the first implantation region and the inner edge of the innermost field limiting ring and the outer edge of the first implantation region.

[0033] A further improvement is that the outer edge of the trench isolation structure located between the inner edge of the stop ring and the outer edge of the outermost field limiting ring is in contact with or has a gap with the inner edge of the stop ring.

[0034] A further improvement is that the semiconductor power device includes a fast recovery diode.

[0035] A further improvement is that, after the second conductive type ion implantation in the first implantation region in step 1, an annealing step is further included;

[0036] After the second conductivity type ion implantation in the second implantation region in step 2, the step of performing annealing is also included.

[0037] A further improvement is that the annealing of the first implantation region and the annealing of the second implantation region are performed simultaneously using the same process.

[0038] The second conductivity type ion implantation in the first implantation region in step one and the second conductivity type ion implantation in the first implantation region in step two are performed separately and independently so that the process structures of the first implantation region and the second implantation region are adjusted independently.

[0039] Alternatively, the second conductivity type ion implantation in the first implantation region in step one and the second conductivity type ion implantation in the first implantation region in step two are combined and performed simultaneously, and step one and step two are combined into one step.

[0040] A further improvement is that the first epitaxial layer is formed on the surface of the semiconductor substrate; after the front process is completed, the following back process is also included:

[0041] Step seven: perform back side thinning to thin the semiconductor substrate to a required thickness.

[0042] Step eight: forming a back electrode region heavily doped with the first conductivity type.

[0043] When the semiconductor substrate is heavily doped with the first conductivity type, the back electrode region is directly formed by the thinned semiconductor substrate.

[0044] Alternatively, the back electrode region is formed by doping the thinned semiconductor substrate with heavily doped impurities of the first conductivity type.

[0045] Step nine: forming a back electrode composed of a back metal layer on the back side of the back electrode region.

[0046] A further improvement is that the first conductivity type is N type and the second conductivity type is P type; or the first conductivity type is P type and the second conductivity type is N type.

[0047] The present invention sets a trench isolation structure between each field limiting ring, and uses the trench isolation structure to restrictively adjust the curved surface of the junction surface of the field limiting ring, that is, the first curved surface, from both sides of the field limiting ring. This can reduce the area of ​​the first curved surface, reduce the corner angles on both sides of the first curved surface, and make the corner positions on both sides of the first curved surface below the top surface of the first epitaxial layer. This can reduce the concentration of electric lines caused by the excessively large corners on both sides of the first curved surface and the concentration of electric lines caused by the corners being located at the top surface of the first epitaxial layer. This can reduce the electric field rise caused by the concentration of electric lines and thereby improve the reverse breakdown voltage of the terminal protection structure. Therefore, the present invention can adjust the curved surface of the junction surface of the field limiting ring, thereby reducing the concentration of electric lines caused by the curved surface corners of the junction surface of the field limiting ring, and can also prevent the electric lines from entering the top surface of the epitaxial layer between the field limiting rings, thereby reducing the electric field rise caused thereby, improving the reverse breakdown voltage of the terminal protection structure and further improving the reverse breakdown voltage of the entire semiconductor power device.

[0048] The formation process of the trench isolation structure of the present invention is placed after the formation process of the first injection region of the main junction and the field limiting ring. The post-placement of the process is conducive to simplification of the process. For example, the first dielectric layer of the trench isolation structure can directly adopt the second oxide layer of the interlayer film, so that the filling process of the trench isolation structure and the deposition process of the interlayer film can be combined, thereby simplifying the process. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:

[0050] Figure 1 is a flow chart of a method for manufacturing a terminal protection structure of a semiconductor power device according to an embodiment of the present invention;

[0051] Figure 2 It is a structural schematic diagram of a terminal protection structure formed by a method for manufacturing a terminal protection structure of a semiconductor power device according to an embodiment of the present invention;

[0052] Figure 3 It is a flow chart of a method for manufacturing a terminal protection structure of a semiconductor power device according to a first preferred embodiment of the present invention;

[0053] Figure 4 It is a flow chart of a method for manufacturing a terminal protection structure of a semiconductor power device according to a second preferred embodiment of the present invention. DETAILED DESCRIPTION

[0054] like Figure 1 FIG. 1 is a flow chart of a method for manufacturing a terminal protection structure of a semiconductor power device according to an embodiment of the present invention; Figure 2 , which is a schematic structural diagram of a terminal protection structure formed by a method for manufacturing a terminal protection structure of a semiconductor power device according to an embodiment of the present invention; Figure 3 FIG. 1 is a flow chart of a method for manufacturing a terminal protection structure of a semiconductor power device according to a first preferred embodiment of the present invention; the method for manufacturing a terminal protection structure of a semiconductor power device according to an embodiment of the present invention comprises the following steps:

[0055] Step 1: provide a first epitaxial layer 102 doped with a first conductivity type, perform second conductivity type ion implantation in a selected region of the first epitaxial layer 102 to form a first implantation region 103; the first implantation region 103 and the first epitaxial layer 102 form a main junction.

[0056] In the method of the first preferred embodiment of the present invention, the first epitaxial layer 102 is formed on the surface of the semiconductor substrate 101 .

[0057] The semiconductor substrate 101 is made of silicon and is epitaxial silicon. Figure 3 In step S101 of the embodiment, in other embodiments, the semiconductor substrate 101 may be a zone melting silicon wafer.

[0058] In the first preferred embodiment of the present invention, before step 1, the method further includes:

[0059] A first conductive type heavily doped ion implantation is performed to form a stop ring 106 in the first epitaxial layer 102 outside the outermost field limiting ring 104. The stop ring 106 is also called a termination ring. Figure 3 As shown, it includes the following steps:

[0060] Step S102 : stop ring photolithography, that is, using a photolithography process to define the formation area of ​​the stop ring 106 .

[0061] In some embodiments, before performing step S102 , the method further includes growing a layer of sacrificial silicon oxide with a thickness of about 50 nm on the first epitaxial layer 102 .

[0062] Step S103, termination ring N injection. In the method of the embodiment of the present invention, the first conductivity type is N type, so the termination ring adopts N type injection, and the termination ring N injection can be implemented by deep N well process to prevent the electric field from diffusing to the chip dicing road. After the injection of the stop ring 106 is completed, annealing is performed, or annealing is performed together with the first injection area 103 in the subsequent step.

[0063] In the first preferred embodiment of the present invention, step 1 includes the following sub-steps:

[0064] Step S106, anode region photolithography, that is, using photolithography to define the first implant region 103. In the embodiment of the present invention, the semiconductor power device is FRD, the first conductivity type is N type, and the second conductivity type is P type, so the first implant region 103 is the anode region of FRD.

[0065] Step S107, P+ implantation and advancement, that is, implantation and annealing advancement are performed on the first implantation region 103, so as to obtain the first implantation region 103. The P+ implantation is implemented by a P-well implantation process.

[0066] Step 2: Perform second conductivity type ion implantation in selected areas of the first epitaxial layer 102 to form multiple second implantation regions, each of which forms a field limiting ring 104; the field limiting ring 104 is a component of a terminal protection structure, and the terminal protection structure surrounds the periphery of the main junction.

[0067] Each field limiting ring 104 is formed in the first epitaxial layer 102 outside the first implantation region 103 and has a ring structure. The radius of the inner edge of each field limiting ring 104 increases from the outer edge of the first implantation region 103 to the outside.

[0068] In the first preferred embodiment of the present invention, step 2 includes the following sub-steps:

[0069] Step S104 : FLR photolithography, that is, using a photolithography process to define the formation area of ​​the FLR 104 .

[0070] Step S105, field limiting ring P implantation and advancement, that is, implantation and annealing advancement of the field limiting ring 104 are performed to obtain the field limiting ring 104. The field limiting ring P implantation is implemented by a P well implantation process.

[0071] In the first preferred embodiment of the present invention, the annealing of the first implantation region 103 and the annealing of the second implantation region are performed simultaneously using the same process. In other embodiments, the annealing of the first implantation region 103 and the annealing of the second implantation region can also be performed separately.

[0072] In the first preferred embodiment of the present invention, the second conductivity type ion implantation of the first implantation region 103 in step 1 and the second conductivity type ion implantation of the first implantation region 103 in step 2 are performed separately and independently so that the process structures of the first implantation region 103 and the second implantation region are independently adjusted. In other embodiments, the second conductivity type ion implantation of the first implantation region 103 in step 1 and the second conductivity type ion implantation of the first implantation region 103 in step 2 can be combined and performed simultaneously; and the annealing of the first implantation region 103 and the annealing of the second implantation region are combined and performed simultaneously using the same process, so that step 1 and step 2 are combined into one step.

[0073] Step three: forming a plurality of first trenches in selected regions of the first epitaxial layer 102; the first trenches are located in a formation region of a terminal protection structure.

[0074] A first dielectric layer is filled in each of the first trenches to form a trench isolation structure 105 .

[0075] In the method of the first preferred embodiment of the present invention, the steps of forming the first trench and the trench isolation structure 105 include:

[0076] A hard mask layer is formed.

[0077] Step S108 is performed, trench photolithography, in which a formation area of ​​the first trench is defined by photolithography, and then the first epitaxial layer 102 is etched to form the first trench.

[0078] Step S109, trench filling / grinding, is performed, and each of the first trenches is filled with a first dielectric layer to form the trench isolation structure 105. Usually, after the first dielectric layer is filled, it will extend to the surface of the area outside the first trench; therefore, it is necessary to planarize the first dielectric layer, for example, by using a chemical mechanical polishing process or an etching back process to remove the first dielectric layer outside the first trench and make the first dielectric layer only in the first trench to form the trench isolation structure 105. The top surface of the first dielectric layer is flush with the top surface of the first epitaxial layer 102 outside the first trench.

[0079] like Figure 2 As shown, the trench isolation structure 105 is formed between the field limiting rings 104 , between the innermost field limiting ring 104 and the first implantation region 103 , and outside the outermost field limiting ring 104 .

[0080] In the first preferred embodiment of the present invention, there is a gap between the inner edge of the trench isolation structure 105 located between the outer edge of the first implantation region 103 and the inner edge of the innermost field limiting ring 104 and the outer edge of the first implantation region 103 .

[0081] The outer edge of the trench isolation structure 105 located between the inner edge of the stop ring 106 and the outer edge of the outermost field limiting ring 104 is in contact with or has a gap with the inner edge of the stop ring 106 .

[0082] Each of the field limiting rings 104 and the first epitaxial layer 102 contacts to form an auxiliary junction; the contact surface of the auxiliary junction is a first curved surface; the trench isolation structure 105 limits the first curved surface from both sides of the first curved surface to reduce the area of ​​the first curved surface, reduce the corner angles on both sides of the first curved surface, and make the corner positions on both sides of the first curved surface located below the top surface of the first epitaxial layer 102, so as to prevent the electric lines at the corners on both sides of the first curved surface from concentrating and make the electric lines away from the top surface of the first epitaxial layer 102 when the semiconductor power device is reverse biased, thereby improving the reverse breakdown voltage of the terminal protection structure.

[0083] In some preferred embodiments, the bottom surface of the first trench is flush with the bottom surface of the field limiting ring 104 to improve the flatness of the depletion layer formed by depletion of each auxiliary junction when the semiconductor power device is reverse biased.

[0084] The following steps are also included:

[0085] Step 4: forming an interlayer film 107.

[0086] The top surface of the trench isolation structure 105 is flush with the top surface of the first epitaxial layer 102 , and the interlayer film 107 is formed on the top surfaces of the trench isolation structure 105 and the first epitaxial layer 102 .

[0087] In the first preferred embodiment of the present invention, step 4 corresponds to Figure 3 Step S110 in the embodiment of the present invention is interlayer dielectric deposition. The interlayer dielectric is the interlayer film 107. The interlayer film 107 is an oxide layer, which is formed by depositing an oxide dielectric layer and densifying the dielectric layer. The effect of humidity and impurities in the external environment on the reverse leakage current of the high-voltage device can be effectively prevented.

[0088] Step 5: forming a contact hole 108 penetrating the interlayer film 107 in a selected area.

[0089] In the first preferred embodiment of the present invention, step five corresponds to Figure 3Step S111, CT lithography and etching; using a lithography process to define the formation area of ​​the contact hole 108, and then etching the interlayer film 107 to form an opening of the contact hole 108 passing through the interlayer film 107.

[0090] Afterwards, the method further includes: step S112 , ion implantation and annealing, for forming a well contact region at the bottom of the opening of the contact hole 108 .

[0091] The contact hole 108 is formed by filling a metal in the opening of the contact hole 108 .

[0092] Step six: forming a front metal layer, and patterning the front metal layer to form a front electrode, wherein the front electrode includes the first electrode 1091 of the main junction and a terminal field plate 1092 .

[0093] The first injection region 103 is connected to the first electrode 1091 through the corresponding contact hole 108 at the top.

[0094] Each of the field limiting rings 104 is connected to the corresponding terminal field plate 1092 through the corresponding contact hole 108 at the top.

[0095] In the first preferred embodiment of the present invention:

[0096] The step of forming the front metal layer corresponds to Figure 3 Step S113, front metal layer deposition.

[0097] The step of patterning the front metal layer corresponds to Figure 3 Step S114, metal photolithography etching, that is, the front metal layer is patterned by using photolithography definition plus metal etching process to form the first electrode 1091 and the terminal field plate 1092 of the main junction.

[0098] After that, it also includes:

[0099] Step S115, photolithography of the front passivation layer. After the front metal layer of the top layer is formed, a passivation layer needs to be formed. The material of the passivation layer includes silicon nitride and polyimide, which is used to protect the semiconductor power device. After that, the passivation layer needs to be patterned using a photolithography definition plus etching process, and the lead-out area of ​​the front metal layer of the top layer is formed in the opening area of ​​the passivation layer. In this way, the production of the top structure is completed.

[0100] Step S116: electron irradiation and annealing.

[0101] The first epitaxial layer 102 is formed on the surface of the semiconductor substrate; after the front process is completed, the following back process is also included:

[0102] Step seven: perform back side thinning to thin the semiconductor substrate to a required thickness.

[0103] Step eight: forming a back electrode region heavily doped with the first conductivity type.

[0104] When the semiconductor substrate is heavily doped with the first conductivity type, the back electrode region is directly formed by the thinned semiconductor substrate.

[0105] Alternatively, the back electrode region is formed by doping the thinned semiconductor substrate with heavily doped impurities of the first conductivity type.

[0106] In the first preferred embodiment of the present invention, step seven and step eight correspond to Figure 3 Step S117 in the back thinning process is to thin the semiconductor substrate 101 to the required thickness, inject N-type impurities into the back, and form a field stop layer by low temperature annealing or laser annealing. The field stop layer also serves as the back electrode region. The semiconductor power device is FRD, so the back electrode region is also the cathode region. At the same time, ensure that the surface impurity concentration is high enough to form an ohmic contact; when the semiconductor substrate 101 with a deep back diffusion layer is selected, the back impurity injection and annealing process may not be performed.

[0107] Step nine: forming a back electrode composed of a back metal layer on the back side of the back electrode region.

[0108] In the first preferred embodiment of the present invention, step nine corresponds to Figure 3 Step S118, back metal, that is, forming a back metal layer on the back of the back electrode region and forming a back electrode composed of the back metal layer. The back metal layer is deposited by sputtering or evaporation, and finally subjected to minority carrier lifetime control process to improve the reverse recovery characteristics of the diode.

[0109] In the first preferred embodiment of the present invention, the semiconductor power device is a fast recovery diode.

[0110] The first conductivity type is N type, and the second conductivity type is P type. At this time, the first injection region 103 is an anode region; the back electrode region is a cathode region. In other embodiments, the first conductivity type can also be P type, and the second conductivity type can be N type.

[0111] Step S119: testing and dicing.

[0112] In the embodiment of the present invention, a trench isolation structure 105 is provided between each field limiting ring 104, and the trench isolation structure 105 is used to restrictively adjust the curved surface of the junction surface of the field limiting ring 104, that is, the first curved surface, from both sides of the field limiting ring 104. This can reduce the area of ​​the first curved surface, reduce the corner angles on both sides of the first curved surface, and make the corner positions on both sides of the first curved surface located below the top surface of the first epitaxial layer 102. This can reduce the concentration of electric lines caused by the excessively large corners on both sides of the first curved surface and the corners located at the top surface of the first epitaxial layer 102. The electric lines of force generated are concentrated, which can reduce the electric field rise caused by the electric line concentration and thus improve the reverse breakdown voltage of the terminal protection structure. Therefore, the embodiment of the present invention can adjust the curved surface of the junction surface of the field limiting ring 104, thereby reducing the electric line concentration caused by the curved surface corner of the junction surface of the field limiting ring 104, and can also prevent the electric lines from entering the top surface of the epitaxial layer between the field limiting rings 104, thereby reducing the electric field rise caused thereby, improving the reverse breakdown voltage of the terminal protection structure and further improving the reverse breakdown voltage of the entire semiconductor power device.

[0113] The formation process of the trench isolation structure 105 of the embodiment of the present invention is placed after the formation process of the first implantation region 103 of the main junction and the field limiting ring 104. The post-placement of the process is not only compatible with the existing process, but also helps to simplify the process.

[0114] like Figure 4 , which is a flow chart of a method for manufacturing a terminal protection structure of a semiconductor power device according to a second preferred embodiment of the present invention; the difference between the method for manufacturing a terminal protection structure of a semiconductor power device according to the second preferred embodiment of the present invention and the method for manufacturing a terminal protection structure of a semiconductor power device according to the first preferred embodiment of the present invention is that in the method for manufacturing a terminal protection structure of a semiconductor power device according to the second preferred embodiment of the present invention:

[0115] In step three, the first dielectric layer is formed by using the interlayer film 107 .

[0116] In step three, after the first trench is formed, the deposition process of the interlayer film 107 in step four is directly performed to form a second oxide layer, which completely fills the first trench and extends to the surface of the outer area of ​​the second oxide layer.

[0117] Afterwards, the second oxide layer is planarized, and the second oxide layer filled in the first trench after planarization forms the trench isolation structure 105; the second oxide layer located on the top of the trench isolation structure 105 and outside the first trench forms the interlayer film 107. The second oxide layer is planarized by chemical mechanical polishing or etching back process.

[0118] Figure 4 In the method, the filling process of the second oxide layer is divided into step S109a, trench / interlayer dielectric deposition; and step S109b, interlayer dielectric deposition. That is, the second oxide layer formed by the interlayer dielectric deposition in step S109a will completely fill the trench, and then the thickness of the second oxide layer needs to be further increased according to the thickness of the interlayer film 107. Then planarization is performed. The second preferred embodiment method of the present invention can further simplify the trench filling process. However, compared with the first preferred embodiment method of the present invention, the quality of the first dielectric layer filling the trench in the second preferred embodiment method of the present invention is limited by the quality of the second oxide layer of the interlayer film 107, and other insulating dielectric materials can also be used. The first preferred embodiment of the present invention can further improve the quality and process flexibility of the trench isolation structure.

[0119] The present invention has been described in detail above through specific embodiments, but these do not constitute a limitation of the present invention. Without departing from the principle of the present invention, those skilled in the art may also make many variations and improvements, which should also be regarded as the protection scope of the present invention.

Claims

1. A method for manufacturing a terminal protection structure of a semiconductor power device, characterized in that: The steps include: Step 1: providing a first epitaxial layer doped with a first conductivity type, and performing second conductivity type ion implantation in a selected region of the first epitaxial layer to form a first implantation region; the first implantation region and the first epitaxial layer form a main junction; Step 2: performing ion implantation of a second conductive type in a selected region of the first epitaxial layer to form a plurality of second implantation regions, each of the second implantation regions forming a field limiting ring; the field limiting ring is a component of a terminal protection structure, and the terminal protection structure surrounds the peripheral side of the main junction; Each of the field limiting rings is formed in the first epitaxial layer outside the first injection region and has a ring structure, and the radius of the inner edge of each of the field limiting rings increases sequentially from the outer edge of the first injection region to the outside; Step 3: forming a plurality of first trenches in a selected region of the first epitaxial layer; the first trenches are located in a formation region of a terminal protection structure; Filling a first dielectric layer in each of the first trenches to form a trench isolation structure; The trench isolation structure is formed between the field limiting rings, between the innermost field limiting ring and the first injection region, and outside the outermost field limiting ring; The field limiting rings and the first epitaxial layer are in contact with each other to form an auxiliary junction; the contact surface of the auxiliary junction is a first curved surface; the trench isolation structure limits the first curved surface from both sides of the first curved surface to reduce the area of ​​the first curved surface, reduce the corner angles on both sides of the first curved surface, and make the corner positions on both sides of the first curved surface below the top surface of the first epitaxial layer, so as to prevent the electric lines at the corners on both sides of the first curved surface from concentrating when the semiconductor power device is reverse biased and make the electric lines away from the top surface of the first epitaxial layer, thereby improving the reverse breakdown voltage of the terminal protection structure; The bottom surface of the first trench is flush with the bottom surface of the field limiting ring, so as to improve the flatness of the depletion layer formed by depletion of each auxiliary junction when the semiconductor power device is reverse biased.

2. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 1, characterized in that: Before step 3, before or after step 1 or step 2, it also includes: A first conductive type heavily doped ion implantation is performed to form a stop ring in the first epitaxial layer outside the outermost field limiting ring.

3. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 2, characterized in that: The following steps are also included: Step 4: forming an interlayer film; The top surface of the trench isolation structure is flush with the top surface of the first epitaxial layer, and the interlayer film is formed on the top surfaces of the trench isolation structure and the first epitaxial layer; Step 5: forming a contact hole through the interlayer film in a selected area; Step 6: forming a front metal layer, and patterning the front metal layer to form a front electrode, wherein the front electrode includes a first electrode of the main junction and a terminal field plate; The first injection region is connected to the first electrode through the corresponding contact hole at the top; Each of the field limiting rings is connected to the corresponding terminal field plate through the corresponding contact hole at the top.

4. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 3, characterized in that: In step three, the first dielectric layer is an oxide layer.

5. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 4, characterized in that: In step three, after the growth of the first dielectric layer is completed, the first dielectric layer completely fills the first trench and also extends to the surface of the outer area of ​​the first trench; After the growth of the first dielectric layer is completed, the first dielectric layer is planarized to completely remove the first dielectric layer outside the first trench and to make the first dielectric layer in the first trench flush with the top surface of the first trench to form the trench isolation structure.

6. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 4, characterized in that: In step three, the first dielectric layer is formed by using the interlayer film; In step 3, after the first trench is formed, the interlayer film deposition process of step 4 is directly performed to form a second oxide layer, which completely fills the first trench and extends to the surface of the outer area of ​​the second oxide layer; Afterwards, the method further includes planarizing the second oxide layer, and the second oxide layer filled in the first trench after planarization forms the trench isolation structure; and the second oxide layer located on the top of the trench isolation structure and outside the first trench forms the interlayer film.

7. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 5, characterized in that: In step three, the first dielectric layer is planarized by chemical mechanical polishing or etching back process.

8. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 6, wherein: In step four, the second oxide layer is planarized by chemical mechanical polishing or etching back process.

9. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 1, characterized in that: There is a distance between the inner edge of the trench isolation structure located between the outer edge of the first implantation region and the inner edge of the innermost field limiting ring and the outer edge of the first implantation region.

10. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 2, characterized in that: The outer edge of the trench isolation structure located between the inner edge of the stop ring and the outer edge of the outermost field limiting ring is in contact with or has a gap with the inner edge of the stop ring.

11. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 1, characterized in that: The semiconductor power device includes a fast recovery diode.

12. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 1, wherein: After the second conductive type ion implantation in the first implantation region in step 1, an annealing step is also included; After the second conductivity type ion implantation in the second implantation region in step 2, the step of performing annealing is also included.

13. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 12, characterized in that: The annealing of the first implantation region and the annealing of the second implantation region are performed simultaneously using the same process; The second conductivity type ion implantation in the first implantation region in step 1 and the second conductivity type ion implantation in the first implantation region in step 2 are performed separately and independently so that the process structures of the first implantation region and the second implantation region are independently adjusted; Alternatively, the second conductivity type ion implantation in the first implantation region in step one and the second conductivity type ion implantation in the first implantation region in step two are combined and performed simultaneously, and step one and step two are combined into one step.

14. The method for manufacturing a terminal protection structure of a semiconductor power device according to claim 3, characterized in that: The first epitaxial layer is formed on the surface of the semiconductor substrate; after the front process is completed, the following back process is also included: Step 7: performing back thinning to thin the semiconductor substrate to a required thickness; Step 8: forming a heavily doped back electrode region of the first conductivity type; When the semiconductor substrate is heavily doped with the first conductivity type, the back electrode region is directly composed of the thinned semiconductor substrate; Alternatively, the back electrode region is formed by doping the thinned semiconductor substrate with heavily doped impurities of the first conductivity type; Step nine: forming a back electrode composed of a back metal layer on the back side of the back electrode region.