A lithium-rich manganese-based positive electrode material and its preparation method and application
By doping B and W elements in the lithium-rich manganese-based positive electrode material, the problems of uneven distribution of Li+ and structural collapse are solved, and the high-rate performance and long-cycle stability of the material are achieved, which significantly improves the capacity retention and rate performance. .
Patent Information
- Application Number
- CN202311142027.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-09-06
AI Technical Summary
Existing lithium-rich manganese-based positive electrode materials are prone to capacity decline and safety problems during long-term circulation, mainly due to the extension of Li+ diffusion path, resulting in uneven distribution of Li+, resulting in cracks and structural collapse in the crystal.
By doping B and W elements respectively during co-precipitation and calcination stages, B elements are uniformly distributed in the crystal to expand the layer spacing. W elements form a stable interface isolation layer during calcination, reducing side reactions during charging and discharging, and enhancing the material structure Stability and cycling performance.
It has achieved good rate performance and long cycle stability. The capacity retention rate of 500 cycles in 1C cycle can reach more than 97.5%, the discharge specific capacity of 0.5C can reach more than 255.1mAh/g, and the discharge specific capacity of 5C can reach more than 210.5mAh/g. The circulation performance and stability of the material are significantly improved.
Smart Images

Figure CN117164019B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries and relates to a lithium-rich manganese-based positive electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-rich manganese-based xLi2MnO3·(1-x)LiMO2 materials have become a hot topic for research and development at home and abroad due to their high capacity (actual discharge capacity exceeds 250mAh / g) and high voltage. The commercially widely used polycrystalline positive electrode allows liquid electrolyte to penetrate into its internal structure, thereby increasing the reaction sites, but it is prone to significant capacity decay and safety issues during long-term cycling.
[0003] Micron-sized single crystal materials can not only effectively alleviate surface and interfacial side reactions in electrochemical processes by reducing the specific surface area, but the reduction of porosity during particle aggregation also helps to increase the compaction density of the positive electrode, showing a higher lithium ion diffusion coefficient.
[0004] CN109956505A discloses a lithium-rich manganese-based positive electrode material and a preparation method and use thereof. The lithium-rich manganese-based positive electrode material is a flexible lithium-rich manganese-based positive electrode material that does not contain other inert components, so that its energy density is significantly improved.
[0005] CN113823786A discloses a method for preparing a modified lithium-rich manganese-based positive electrode material, wherein a single crystal fast lithium ion conductor coated lithium-rich manganese-based positive electrode material is obtained by simultaneously performing single crystal and surface coating treatment by ball milling.
[0006] Diffusion distance and diffusion coefficient play a joint role in capacity. One disadvantage of the single crystal positive electrode material described in the above scheme is that Li + The diffusion path is extended, resulting in Li + The uneven distribution eventually leads to cracks inside the crystal after long-term cycling at high voltage or high current density. In addition, when the positive electrode is cycled in a highly delithiated state, it undergoes an irreversible phase transition from H2 to H3, resulting in a sudden contraction of the lattice and the generation of nanocracks. Once cracks begin to form, capacity decay occurs. Summary of the invention
[0007] The object of the present invention is to provide a lithium-rich manganese-based positive electrode material and a preparation method and application thereof. The present invention is directed to the action principle of the doping element, and doping is performed separately in the coprecipitation stage and the calcination stage to maximize the effect of doping modification. By uniformly doping the B element inside the single crystal, the interlayer spacing is expanded, which is beneficial to lithium ion transmission and a stable crystal structure is achieved; by doping the W element, a stable interface is formed, which alleviates the gas production and structural collapse caused by the reaction of oxygen-containing components with the electrolyte. Through material modification, good rate performance and long cycle stability can be achieved.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing a lithium-rich manganese-based positive electrode material, the preparation method comprising the following steps:
[0010] (1) mixing a nickel source, a manganese source and a boron source with a solvent to obtain a mixed salt solution, and adding the mixed salt solution, an alkali solution and an ammonia solution to a base liquid in parallel for a co-precipitation reaction to obtain a boron-doped positive electrode precursor;
[0011] (2) calcining the boron-doped positive electrode precursor to obtain an oxide;
[0012] (3) The oxide, tungsten source and lithium source are mixed, and the mixture is sintered to obtain the lithium-rich manganese-based positive electrode material.
[0013] The present invention adds B element in the coprecipitation process so that it can be evenly distributed in the crystal, thereby enhancing the structural stability of the material; and adds W element in the lithiation calcination stage so that an isolation layer is formed on the particle surface during calcination, thereby reducing side reactions in the charge and discharge process and improving the cycle performance of the material.
[0014] Preferably, the nickel source in step (1) comprises any one of nickel chloride, nickel sulfate or nickel nitrate, or a combination of at least two of them.
[0015] Preferably, the manganese source includes any one of manganese chloride, manganese sulfate or manganese nitrate, or a combination of at least two of them.
[0016] Preferably, the boron source comprises boron oxide and / or boric acid.
[0017] Preferably, the molar ratio of the total molar amount of the nickel source and the manganese source to the boron element in the boron source is (99.5-99.98):(0.02-0.5), for example: 99.98:0.02, 99.95:0.05, 99.9:0.1, 99.7:0.3 or 99.5:0.5, etc.
[0018] Preferably, the total molar concentration of nickel and manganese in the mixed salt solution of step (1) is 1 to 3 mol / L, for example: 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L or 3 mol / L.
[0019] Preferably, the alkali solution comprises sodium hydroxide solution and / or potassium hydroxide solution.
[0020] Preferably, the concentration of the alkali solution is 8-10 mol / L, for example, 8 mol / L, 8.5 mol / L, 9 mol / L, 9.5 mol / L or 10 mol / L.
[0021] Preferably, the concentration of the ammonia water is 8-10 mol / L, for example, 8 mol / L, 8.5 mol / L, 9 mol / L, 9.5 mol / L or 10 mol / L.
[0022] Preferably, the temperature of the coprecipitation reaction in step (1) is 40-80°C, for example, 40°C, 50°C, 60°C, 70°C or 80°C.
[0023] Preferably, the pH of the coprecipitation reaction is 8-12, for example, 8, 9, 10, 11 or 12.
[0024] Preferably, the temperature of the calcination treatment in step (2) is 600-950°C, for example, 600°C, 700°C, 800°C, 900°C or 950°C.
[0025] Preferably, the calcination treatment time is 6 to 10 hours, for example: 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.
[0026] Preferably, the tungsten source in step (3) comprises WO3.
[0027] Preferably, the molar ratio of the oxide to the tungsten source is 100:(0.02-0.5), for example: 100:0.02, 100:0.05, 100:0.1, 100:0.3 or 100:0.5, etc.
[0028] Preferably, the lithium source comprises lithium hydroxide and / or lithium carbonate.
[0029] Preferably, the temperature of the sintering treatment in step (3) is 900-1000°C, for example, 900°C, 920°C, 950°C, 980°C or 1000°C.
[0030] Preferably, the sintering treatment time is 6 to 10 hours, for example: 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.
[0031] In a second aspect, the present invention provides a lithium-rich manganese-based positive electrode material, which is prepared by the method described in the first aspect.
[0032] In the lithium-rich manganese-based positive electrode material of the present invention, B occupies the tetrahedral interstitial position of the oxygen-filled lattice, forming a stronger BO covalent bond, blocking the migration channel of the transition metal ions, and the uniform distribution of the B element inside the crystal can achieve an ideal stable structure, effectively alleviating the concentration gradient distribution of lithium ions in micron-sized single crystals, causing serious lattice mismatch between the bulk phase and the surface, and the accumulation of micro-stress strain in the grains. W is added together with the lithium source during lithiation calcination, and no additional synthesis process is added. W reacts with the lithium source during the heat treatment process to form a LWO layer on the surface of the single crystal, which helps to improve the mechanical strength. The charge accumulation around W is greater than that of Ni, forming a WO bond stronger than Ni-O, strengthening the interface and improving the surface stability.
[0033] In a third aspect, the present invention provides a positive electrode plate, wherein the positive electrode plate comprises the lithium-rich manganese-based positive electrode material as described in the second aspect.
[0034] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the positive electrode sheet as described in the third aspect.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The present invention aims at the working principle of the doping elements, and performs doping respectively in the coprecipitation stage and the calcination stage to maximize the effect of doping modification. By uniformly doping the B element inside the single crystal, the interlayer spacing is expanded, which is beneficial to lithium ion transmission and a stable crystal structure is achieved; by doping the W element, a stable interface is formed, which alleviates the gas production and structural collapse caused by the reaction of oxygen-containing components with the electrolyte. Through material modification, good rate performance and long cycle stability can be achieved.
[0037] (2) The capacity retention rate of the battery made of the lithium-rich manganese-based positive electrode material of the present invention after 500 cycles at 1C can reach more than 97.5%, the 0.5C discharge specific capacity can reach more than 255.1mAh / g, the 1C discharge specific capacity can reach more than 245.6mAh / g, the 2C discharge specific capacity can reach more than 226.3mAh / g, the 5C discharge specific capacity can reach more than 210.5mAh / g, and the 10C discharge specific capacity can reach more than 187.1mAh / g. The co-doping of appropriate amounts of metal W and non-metal B can stabilize the material structure and improve the transmission of lithium ions. The material performance is judged by preparing different lithium-rich manganese-based positive electrode materials. The test is simple and the results are highly reliable, which proves that the performance is best when the appropriate doping amounts of W and B are used. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a SEM image of the lithium-rich manganese-based positive electrode material described in Example 1 of the present invention. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0040] Example 1
[0041] This embodiment provides a lithium-rich manganese-based positive electrode material, and the preparation method of the lithium-rich manganese-based positive electrode material is as follows:
[0042] (1) nickel salt, manganese salt and boron compound are prepared into a mixed salt solution according to the stoichiometric ratio of Ni:Mn:B=0.249:0.75:0.001, and 10 mol / L of liquid alkali solution and 9 mol / L of ammonia water are prepared. Under nitrogen protection, the mixed salt solution, alkali solution and ammonia water are respectively added to a reactor through a metering pump, and a coprecipitation reaction is carried out at 45° C. and pH 11. When the average particle size of the material in the reactor reaches 4 μm, the feeding is stopped, the solution in the reactor is centrifuged and washed, and dried to obtain a B-doped lithium-rich manganese-based positive electrode precursor;
[0043] (2) placing the prepared precursor in a calcining furnace at 650° C. for 6 h to obtain the corresponding oxide;
[0044] (3) The above-mentioned precursor oxide is mixed with WO3 and lithium source at a molar ratio of oxide: W:Li = 1:0.001:1.15 at high speed, and then calcined at 970°C in a sintering furnace for 8 hours to obtain the lithium-rich manganese-based positive electrode material. The SEM image of the lithium-rich manganese-based positive electrode material is as follows Figure 1 shown.
[0045] Example 2
[0046] This embodiment provides a lithium-rich manganese-based positive electrode material, and the preparation method of the lithium-rich manganese-based positive electrode material is as follows:
[0047] (1) nickel salt, manganese salt and boron compound are prepared into a mixed salt solution according to the stoichiometric ratio of Ni:Mn:B=0.2498:0.75:0.0002, and 9 mol / L of liquid alkali solution and 8 mol / L of ammonia water are prepared. Under nitrogen protection, the mixed salt solution, alkali solution and ammonia water are respectively added to a reactor through a metering pump, and a coprecipitation reaction is carried out at 45° C. and pH 11. When the average particle size of the material in the reactor reaches 4 μm, the feeding is stopped, the solution in the reactor is centrifuged and washed, and dried to obtain a B-doped lithium-rich manganese-based positive electrode precursor;
[0048] (2) placing the prepared precursor in a calcining furnace at 600° C. for 6 h to obtain the corresponding oxide;
[0049] (3) The above-mentioned precursor oxide is mixed with WO3 and a lithium source at a molar ratio of oxide: W:Li=1:0.0002:1.12 at a high speed, and then calcined at 900°C in a sintering furnace for 10 hours to obtain the lithium-rich manganese-based positive electrode material.
[0050] Example 3
[0051] This embodiment provides a lithium-rich manganese-based positive electrode material, and the preparation method of the lithium-rich manganese-based positive electrode material is as follows:
[0052] (1) nickel salt, manganese salt and boron compound are prepared into a mixed salt solution according to the stoichiometric ratio of Ni:Mn:B=0.245:0.75:0.005, and 10 mol / L of liquid alkali solution and 9 mol / L of ammonia water are prepared. Under nitrogen protection, the mixed salt solution, alkali solution and ammonia water are respectively added to a reactor through a metering pump, and a coprecipitation reaction is carried out at 45° C. and pH 11. When the average particle size of the material in the reactor reaches 4 μm, the feeding is stopped, the solution in the reactor is centrifuged and washed, and dried to obtain a B-doped lithium-rich manganese-based positive electrode precursor;
[0053] (2) placing the prepared precursor in a calcining furnace at 950° C. for 6 h to obtain the corresponding oxide;
[0054] (3) The above-mentioned precursor oxide is mixed with WO3 and a lithium source at a molar ratio of oxide: W:Li = 1:0.001:1.15 at a high speed, and then calcined at 1000° C. for 6 hours in a sintering furnace to obtain the lithium-rich manganese-based positive electrode material.
[0055] Example 4
[0056] The only difference between this embodiment and embodiment 1 is that the molar ratio of the total molar amount of the nickel source and the manganese source to the boron element in the boron source is 99:1, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0057] Example 5
[0058] The only difference between this embodiment and embodiment 1 is that the molar ratio of the total molar amount of the nickel source and the manganese source to the boron element in the boron source is 99.99:0.01, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0059] Example 6
[0060] The only difference between this embodiment and embodiment 1 is that the molar ratio of the oxide to the tungsten source is 99:1, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0061] Example 7
[0062] The only difference between this embodiment and embodiment 1 is that the molar ratio of oxide to tungsten source is 99.99:0.01, and other conditions and parameters are exactly the same as those in embodiment 1.
[0063] Comparative Example 1
[0064] The only difference between this comparative example and Example 1 is that boron and tungsten are directly doped by co-precipitation, and other conditions and parameters are exactly the same as those in Example 1.
[0065] Comparative Example 2
[0066] The only difference between this comparative example and Example 1 is that no boron source is added, and other conditions and parameters are exactly the same as those in Example 1.
[0067] Example 3
[0068] The only difference between this comparative example and Example 1 is that no tungsten source is added, and other conditions and parameters are exactly the same as those in Example 1.
[0069] Performance Testing:
[0070] The first week charge and discharge specific capacity and cycle performance use constant current charge and discharge mode to charge and discharge button cells at room temperature. The positive electrode material is assembled into a CR2025 button cell, and the charge and discharge cycle is performed for 100 cycles at 25°C, the voltage range is 2.5V~4.6V, and 1C / 1C. Test method for rate performance: The rate performance of the battery is tested using 0.5C, 1C, 2C, 5C and 10C current densities. The test results are shown in Table 1:
[0071] Table 1
[0072]
[0073] As can be seen from Table 1, from Examples 1-3, the capacity retention rate of the battery made of the lithium-rich manganese-based positive electrode material of the present invention after 1C cycle 500 cycles can reach more than 97.5%, the 0.5C discharge specific capacity can reach more than 255.1 mAh / g, the 1C discharge specific capacity can reach more than 245.6 mAh / g, the 2C discharge specific capacity can reach more than 226.3 mAh / g, the 5C discharge specific capacity can reach more than 210.5 mAh / g, and the 10C discharge specific capacity can reach more than 187.1 mAh / g. The B and W co-doped lithium-rich manganese-based positive electrode materials with appropriate content ranges in stages of the present invention show excellent capacity retention and rate performance.
[0074] By comparing Example 1 with Examples 4-5, it can be seen that in the lithium-rich manganese-based positive electrode material of the present invention, the amount of boron doping will affect its performance. During the preparation process, the molar ratio of the total molar amount of the nickel source and the manganese source to the boron element in the boron source is controlled at (99.5-99.98): (0.02-0.5). The performance of the lithium-rich manganese-based positive electrode material is good. If the boron doping amount is too large, the transitional substitution of boron in the crystal structure will affect the performance of the transition metal capacity and even cause lattice distortion. If the boron doping amount is too small, the effect of widening the lithium ion channel cannot be achieved, and there is no obvious improvement on the diffusion and migration of lithium ions, and the capacity will also be limited.
[0075] By comparing Example 1 with Examples 6-7, it can be seen that in the lithium-rich manganese-based positive electrode material of the present invention, the amount of tungsten doping will affect its performance. During the preparation process, the molar ratio of the oxide to the tungsten source is controlled at 100:(0.02-0.5), and the performance of the lithium-rich manganese-based positive electrode material is good. If the tungsten doping amount is too large, the crystal internal resistance will increase, which will deteriorate the cycle performance of the material and also make the rate performance worse; if the tungsten doping amount is too small, there is not enough W diffused to the crystal surface to form a stable isolation layer, and the effect of improving the cycle performance cannot be achieved.
[0076] By comparing Example 1 and Comparative Example 1, it can be seen that the present invention adds the B element during the coprecipitation process so that it can be evenly distributed in the crystal, thereby enhancing the structural stability of the material; and by adding the W element during the lithiation calcination stage, an isolation layer is formed on the surface of the particles during calcination, thereby reducing side reactions during the charge and discharge process and improving the cycle performance of the material.
[0077] By comparing Example 1 with Comparative Examples 2-3, it can be seen that in the lithium-rich manganese-based positive electrode material of the present invention, B occupies the tetrahedral gap position of the oxygen-filled lattice, forming a stronger BO covalent bond, blocking the migration channel of the transition metal ions, and the uniform distribution of the B element inside the crystal can achieve an ideal stable structure, effectively alleviating the concentration gradient distribution of lithium ions in micron-sized single crystals, causing serious lattice mismatch between the bulk phase and the surface, and the accumulation of microstress strain in the grains. W is added together with the lithium source during lithiation calcination, and no additional synthesis process is added. W reacts with the lithium source during the heat treatment process to form a LWO layer on the surface of the single crystal, which helps to improve the mechanical strength. The charge accumulation around W is greater than that of Ni, forming a stronger WO bond than Ni-O, strengthening the interface and improving the surface stability.
[0078] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a lithium-rich manganese-based positive electrode material, characterized in that: The preparation method comprises the following steps: (1) mixing a nickel source, a manganese source and a boron source with a solvent to obtain a mixed salt solution, and adding the mixed salt solution, an alkali solution and an ammonia solution to a base liquid in parallel for a co-precipitation reaction to obtain a boron-doped positive electrode precursor; (2) calcining the boron-doped positive electrode precursor to obtain an oxide; (3) mixing the oxide, tungsten source and lithium source, and sintering to obtain the lithium-rich manganese-based positive electrode material; The alkali solution in step (1) includes sodium hydroxide solution and / or potassium hydroxide solution; The molar ratio of the oxide to the tungsten source in step (3) is 100:(0.02-0.5); The molar ratio of the total molar amount of the nickel source and the manganese source in step (1) to the boron element in the boron source is (99.5~99.98):(0.02~0.5).
2. The preparation method according to claim 1, characterized in that The nickel source in step (1) includes any one of nickel chloride, nickel sulfate or nickel nitrate, or a combination of at least two of them.
3. The preparation method according to claim 1, characterized in that: The manganese source in step (1) includes any one of manganese chloride, manganese sulfate or manganese nitrate, or a combination of at least two of them.
4. The preparation method according to claim 1, characterized in that: The boron source in step (1) includes boron oxide and / or boric acid.
5. The preparation method according to claim 1, characterized in that: The total molar concentration of nickel and manganese in the mixed salt solution of step (1) is 1-3 mol / L.
6. The preparation method according to claim 1, characterized in that: The concentration of the alkali solution is 8-10 mol / L.
7. The preparation method according to claim 1, characterized in that: The concentration of the ammonia water in step (1) is 8-10 mol / L.
8. The preparation method according to claim 1, characterized in that: The temperature of the coprecipitation reaction in step (1) is 40-80°C.
9. The preparation method according to claim 1, characterized in that: The pH of the coprecipitation reaction in step (1) is 8-12.
10. The preparation method according to claim 1, characterized in that: The temperature of the calcination treatment in step (2) is 600-950°C.
11. The preparation method according to claim 1, characterized in that: The calcination time in step (2) is 6 to 10 hours.
12. The preparation method according to claim 1, characterized in that: The tungsten source in step (3) includes WO3.
13. The preparation method according to claim 1, characterized in that: The lithium source in step (3) includes lithium hydroxide and / or lithium carbonate.
14. The preparation method according to claim 1, characterized in that: The sintering temperature in step (3) is 900-1000°C.
15. The preparation method according to claim 1, characterized in that: The sintering time in step (3) is 6 to 10 hours.
16. A lithium-rich manganese-based positive electrode material, characterized in that: The lithium-rich manganese-based positive electrode material is prepared by the method according to any one of claims 1 to 15.
17. A positive electrode plate, characterized in that: The positive electrode plate comprises the lithium-rich manganese-based positive electrode material as claimed in claim 16.
18. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet as claimed in claim 17.
Citation Information
Patent Citations
Lithium-rich manganese-based positive electrode material, and preparation method and use thereof
CN109956505A
Modified lithium-rich manganese-based positive electrode material and preparation method thereof
CN113823786A
A tungsten ion doped high-nickel layered oxide lithium electrode material and a preparation method thereof
CN109167056A
Modified boron-doped lithium-rich manganese-based anode material, and preparation method and application thereof
CN110429268A
Preparation method of lithium-rich manganese-based positive electrode material
CN111170377A