A kind of Bi 19 S 27 Br3 / CoAl-LDH composite photocatalyst and its preparation method and application
Through the composite material of Bi19S27Br3 and CoAl-LDH, the S-shaped heterojunction is formed, which solves the problem of low charge transfer efficiency of the photocatalyst, significantly improves the photocatalytic activity and CO2 reduction performance, and achieves a more efficient photocatalytic effect.
Patent Information
- Application Number
- CN202311229762.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-09-22
AI Technical Summary
The charge transfer efficiency of the photocatalyst is low, resulting in a short electron-hole recombination life during the photocatalysis process, which affects the photocatalytic effect.
A composite material of Bi19S27Br3 and CoAl-LDH was used to combine Bi19S27Br3 nanorods with CoAl-LDH by solvothermal method to form an S-shaped heterojunction, which improves the charge carrier separation rate and light absorption capacity of the photocatalyst.
The photocatalytic activity and stability of the photocatalyst are significantly enhanced, the CO2 reduction performance is improved, the electron-hole recombination life is extended, and the photocatalytic reduction performance is improved.
Smart Images

Figure HDA0004463495580000011 
Figure HDA0004463495580000012 
Figure HDA0004463495580000021
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of composite photocatalysts and particularly relates to a Bi 19 S 27 Br3 / CoAl-LDH composite photocatalyst, preparation method and application thereof. Background Art
[0002] As global warming intensifies, the content of greenhouse gases such as carbon dioxide has increased, which is an important factor in global ecological destruction. Photocatalytic technology is not only an effective way to solve the high content of carbon dioxide in the atmosphere, but also environmentally friendly. However, the difficulty of photocatalytic technology lies in the low charge transfer efficiency of photocatalysts. Therefore, introducing electron accumulation materials and direct S-type heterojunction on the surface of photocatalysts is considered to be an effective method.
[0003] As a metal sulfide halide, Bi 19 S 27 Br3 has excellent electrical conductivity, high light absorption capacity, and a sufficiently negative conduction band (CB) position, which ensures strong reduction ability for photoexcited electrons. 19 S 27 Br3 shows great application prospects in CO2 photoreduction research.
[0004] Layered double hydroxides (LDHs) are interesting clay minerals composed of mixed metal oxides. Their unique layered structure has inspired their application in many fields. Specifically, oxygen bridges can suppress electron-hole recombination through metal-metal charge transfer mechanisms. For example, CeO2 nanoparticles dispersed on CoAl-LDH nanosheets were used for composite photocatalytic hydrogen evolution. Alternatively, sulfadiazine was photocatalytically degraded by self-assembled CoAl-LDH / g-C3N4 heterostructures. However, due to the short lifetime of the generated electron-hole pairs, LDH has a mediocre effect in the photocatalytic process. Therefore, LDH and Bi were chosen to be combined. 19 S 27 The combination of Br3 may solve these shortcomings. Summary of the invention
[0005] Based on the above analysis, the present invention designed and synthesized Bi 19 S 27 Br3 / CoAl-LDH composite material. Bi in this photocatalytic system 19 S 27 Br3 acts as an electron accumulation active site to extract photogenerated electrons on the surface of CoAl-LDH and effectively activate CO2 molecules.
[0006] The object of the present invention is to provide a composite material having an S-type heterojunction, namely Bi19 S 27 Br3 / CoAl-LDH and its preparation method and performance research, the prepared photocatalyst effectively inhibits the recombination of photogenerated electron-hole pairs, has good visible light photocatalytic activity, and also has a large specific surface area.
[0007] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions:
[0008] The present invention 19 S 27 Preparation method of Br3 / CoAl-LDH composite material, Bi 19 S 27 Br3 nanorods were combined with CoAl-LDH to synthesize the photocatalytic material Bi 19 S 27 Br3 / CoAl-LDH, specifically comprising the following steps:
[0009] (1) Dissolve Co(NO3)2·9H2O and Al(NO3)3·9H2O in deionized water and add a certain amount of Bi 19 S 27 Br3 and disperse it in the above solution.
[0010] (2) Then add NaOH and Na2CO3 to the suspension and stir for another 30 minutes. Stir with ultrasound until it turns completely black. Place the obtained suspension in a polytetrafluoroethylene liner and heat at 120-130°C for 16-17 hours.
[0011] (3) After cooling to room temperature, the material was washed with ethanol and deionized water and dried at 60 °C. The composite material was labeled as X-Bi 19 S 27 Br3 / CoAl-LDH (X = 33, 50 and 66%), where X is Bi in the composite material 19 S 27 Mass percentage of Br3.
[0012] The crystalline phase of the material was recorded by using a D / MAX2500 diffractometer (Rigaku, Japan) to obtain an X-ray diffraction (XRD) pattern. Ultraviolet visible (Uv-vis) diffuse reflectance spectra (DRS) were recorded using Shimadzu Uv-2550. The PL spectra of the samples were detected using an Edinburgh FL / FS900 spectrophotometer. X-ray photoelectron spectroscopy (XPS) analysis was performed on the chemical composition and valence state using an ESCALAB 250Xi analyzer. Micromorphology was analyzed using a transmission electron microscope (TEM) and a scanning electron microscope (SEM) combined with an energy dispersive spectroscopy (EDS).
[0013] The present invention also provides the above-mentioned Bi 19 S 27 Application of Br3 / CoAl-LDH composite photocatalyst, the Bi 19 S 27 The Br3 / CoAl-LDH composite photocatalyst is used for visible light catalytic carbon dioxide reduction. It includes the following steps: deionized water, sacrificial agent and Bi 19 S 27 The Br3 / CoAl-LDH composite material was added into the photoreactor and reacted under a CO2 gas atmosphere at normal pressure.
[0014] The beneficial effect of the present invention is: using the solvent thermal method to synthesize Bi 19 S 27 Br3 / CoAl-LDH composite material is a photocatalytic material with an attached structure. 19 S 27 The combination of Br3 and CoAl-LDH has a stronger charge carrier separation rate and reduces the recombination rate of electrons and holes; it significantly enhances the photogenerated charge transfer and increases the light absorption capacity, thereby improving the performance of photocatalytic reduction of CO2. The material has the advantages of high photocatalytic reduction performance and good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 for Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 XRD and IR spectra images of Br3 / CoAl-LDH;
[0016] Figure 2 for Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 SEM image, TEM image and mapping diagram of Br3 / CoAl-LDH;
[0017] Figure 3 for Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 XPS spectrum of Br3 / CoAl-LDH;
[0018] Figure 4 for Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S27 CO (a) and CH4 (b) production graphs of Br3 / CoAl-LDH;
[0019] Figure 5 for 66-Bi 19 S 27 Cycling experiment of Br3 / CoAl-LDH and XRD pattern of the material after the cycling experiment;
[0020] Figure 6 for Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 PL pattern of Br3 / CoAl-LDH;
[0021] Figure 7 for Bi 19 S 27 Br3, CoAl-LDH and X-Bi 19 S 27 UV-Vis DRS of Br3 / CoAl-LDH;
[0022] Figure 8 for Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 Electrochemical diagram of Br3 / CoAl-LDH;
[0023] Fig. 9 for Bi 19 S 27 Bandgap width of Br3 and CoAl-LDH, XPS spectrum, Mott-Schottky spectrum;
[0024] Fig.10 for Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 ESR graph of Br3 / CoAl-LDH. DETAILED DESCRIPTION
[0025] The present invention is described in detail below in conjunction with the embodiments so that those skilled in the art can better understand the present invention, but the present invention is not limited to the following embodiments.
[0026] Example 1
[0027] (1)Bi 19 S 27 Preparation of Br3:
[0028] A. Disperse thiourea (0.5 mmol), [C16mim]Br (0.4 mmol) and Bi(NO3)3·5H2O (0.02 mmol) in 20 mL of ethylene glycol and sonicate for 30 min to form a uniformly dispersed solution;
[0029] B. After stirring the mixture for 30 minutes, the mixture was transferred to a 150 mL polytetrafluoroethylene-lined autoclave and heated at 130°C for 12 hours. The resulting black powder was washed several times with deionized water and ethanol and vacuum dried at 60°C for 24 hours to obtain Bi 19 S 27 Br3.
[0030] (2)66-Bi 19 S 27 Preparation of Br3 / CoAl-LDH composite materials:
[0031] Co(NO3)2·9H2O (1 mmol) and Al(NO3)3·9H2O (0.5 mmol) were dissolved in 50 mL of deionized water and Bi 19 S 27 Br3 (5 mmol) was added and dispersed in the above solution. Then (4 mmol) NaOH and Na2CO3 (1.5 mmol) were added to the suspension and stirred for another 30 minutes. Ultrasonic stirring was performed until it turned completely black. The obtained suspension was placed in a 150 mL polytetrafluoroethylene liner and heated at 120°C for 16 hours. After cooling to room temperature, the material was washed with ethanol and deionized water and dried at 60°C. The resulting composite material was labeled as 66-Bi 19 S 27 Br3 / CoAl-LDH composite materials.
[0032] Example 2
[0033] (1)Bi 19 S 27 Preparation of Br3: Same as Example 1;
[0034] (2) 50-Bi 19 S 27 Preparation of Br3 / CoAl-LDH composite materials:
[0035] Co(NO3)2·9H2O (1 mmol) and Al(NO3)3·9H2O (0.5 mmol) were dissolved in 50 mL of deionized water and Bi 19 S 27Br3 (3 mmol) was added and dispersed in the above solution. Then (4 mmol) NaOH and Na2CO3 (1.5 mmol) were added to the suspension and stirred for another 30 minutes. Ultrasonic stirring was performed until it turned completely black. The obtained suspension was placed in a 150 mL polytetrafluoroethylene liner and heated at 120 ° C for 16 hours. After cooling to room temperature, the material was washed with ethanol and deionized water and dried at 60 ° C to obtain 50-Bi 19 S 27 Br3 / CoAl-LDH composite materials.
[0036] Example 3
[0037] (1)Bi 19 S 27 Preparation of Br3: Same as Example 1;
[0038] (2)33-Bi 19 S 27 Preparation of Br3 / CoAl-LDH composite materials:
[0039] Co(NO3)2·9H2O (1 mmol) and Al(NO3)3·9H2O (0.5 mmol) were dissolved in 50 mL of deionized water and Bi 19 S 27 Br3 (2 mmol) was added and dispersed in the above solution. Then (4 mmol) NaOH and Na2CO3 (1.5 mmol) were added to the suspension and stirred for another 30 minutes. Ultrasonic stirring was performed until it turned completely black. The obtained suspension was placed in a 150 mL polytetrafluoroethylene liner and heated at 120 ° C for 16 hours. After cooling to room temperature, the material was washed with ethanol and deionized water and dried at 60 ° C to obtain 33-Bi 19 S 27 Br3 / CoAl-LDH composite materials.
[0040] The present invention also synthesized CoAl-LDH for comparison, and its preparation method is as follows:
[0041] A. Dissolve Co(NO3)2·9H2O (1 mmol) and Al(NO3)3·9H2O (0.5 mmol) in 50 mL of deionized water, and name the mixed solution Solution A;
[0042] B. Then weigh NaOH (4 mmol) and Na2CO3 (1.5 mmol) and disperse them in 15 mL of solution B;
[0043] C. After 5 minutes of magnetic stirring, solution A was added dropwise to solution B. The pink solution was transferred to a 150 mL polytetrafluoroethylene-lined autoclave and kept at 120 °C for 16 hours in the autoclave. Then, the reacted sample was placed in a centrifuge tube, washed several times with deionized water and ethanol in a high-speed centrifuge, and transferred to an oven and dried at 60 °C overnight. Finally, CoAl-LDH was obtained by grinding in an agate mortar.
[0044] XRD analysis of Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 Crystal structure of Br3 / CoAl-LDH ( Figure 1 a). For CoAl-LDH, the typical diffraction peaks at 11.6°, 23.4°, 34.7°, 61.7° and 62.2° correspond to the (003), (006), (009), (110) and (113) crystal planes of hexagonal CoAl-LDH (JCPDS: 51-0045). 19 S 27 All diffraction peaks of Br3 and Bi 19 S 27 The Br3 standard matches (JCPDS: 26-0813). 19 S 27 In the scaled diffraction pattern of Br3 / CoAl-LDH, all the diffraction peaks correspond to Bi 19 S 27 The characteristic peaks of Br3 and CoAl-LDH prove that Bi 19 S 27 The success of the combination of Br3 and CoAl-LDH.
[0045] Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 FT-IR spectrum of Br3 / CoAl-LDH ( Figure 1 b). Observed 3600-3000cm -1 The broad band in the region is assigned to the vibration mode of the OH group. For CoAl-LDH, 1633 cm -1 The weak band at 1346 cm is due to the stretching vibration of interlayer H2O, while the -1 and 820cm -1 The peak at is due to CO3 2- In addition, 554cm -1 and 610cm -1The weak peaks of Bi 19 S 27 Br3 and CoAl-LDH showed similar 19 S 27 Br3 / CoAl-LDH similar bands, indicating that the prepared heterojunction retains Bi 19 S 27 The structures of Br3 and CoAl-LDH, and the material surface has a large number of hydroxyl functional groups.
[0046] The morphology, structure and elements of the samples were analyzed by scanning electron microscopy, transmission electron microscopy and energy dispersive spectrometer ( Figure 2 ). SEM can observe Bi 19 S 27 Br3 presents a 5μm rod-like structure ( Figure 2 a). CoAl-LDH exhibits a hexagonal sheet structure with a diameter of about 500 nm ( Figure 2 b). It can be seen that Figure 2 In c, the rod-shaped material and the flake-shaped material are closely combined. The stripes with lattice spacing of 0.314nm and 0.796nm correspond to Bi 19 S 27 The (211) crystal plane of Br3 and the (003) crystal plane of CoAl-LDH. 19 S 27 Elemental analysis of the Br3 / CoAl LDH catalyst revealed that only signals belonging to Co, Al, O, Br, Bi, and S were detected ( Figure 2 gm), indicating that 66-Bi 19 S 27 There are no impurities in Br3 / CoAl-LDH. This indicates that 66-Bi 19 S 27 Br3 / CoAl-LDH composites have been successfully prepared.
[0047] XPS was used to study the chemical composition and state of the photocatalyst, as well as Bi 19 S 27 The interaction between Br3 and CoAl-LDH. Figure 3 a, in 66-Bi 19 S 27 Characteristic peaks of Co, Al, O, Bi, S and Br elements were detected in the Br3 / CoAl-LDH composite material. Figure 3 b, observed Bi 19 S 27 Br3 has two peaks at 158.09eV and 163.24eV, corresponding to Bi3+ Bi 4f ions 7 / 2 and Bi 4f 5 / 2 The peaks overlapping with Bi4f at 160.66 eV and 161.89 eV are attributed to S 2- S2p of ions 3 / 2 and S2p 1 / 2 . with Bi 19 S 27 Compared with Br3, 66-Bi 19 S 27 The binding energy of Br3 / CoAl-LDH shifted negatively. Figure 3 As shown in c, the signal with a binding energy of 67.36 eV is characteristic of Br ions (Br 3d). 19 S 27 The signal of Br3 / CoAl-LDH (67.08 eV) and Bi 19 S 27 Br3 also shows a negative shift. Figure 3 In e, the characteristic peak at 74.10 eV belongs to Al 2p, indicating that Al in CoAl-LDH 3+ ions. In 66-Bi 19 S 27 In the Br3 / CoAl-LDH complex, the Al 2p peak (74.25 eV) shows a significant positive shift. Figure 3 d), CoAl-LDH has two peaks at about 531.30 eV and 531.70 eV, corresponding to Co-O and Al-O. Figure 3 As shown in f, the Co 2p peaks of CoAl-LDH at 781.11 eV and 797.12 eV belong to Co 2p 3 / 2 and Co 2p 1 / 2 The presence of two satellite peaks indicates that CoAl-LDH contains high-spin divalent Co 2+ According to the changes in element composition and binding energy, Bi 19 S 27 A close interaction is formed between Br3 and CoAl-LDH, which is beneficial to the transfer of photogenerated charges.
[0048] The photocatalytic activity experiment was carried out at room temperature and atmospheric pressure. The test was carried out by bubbling method. 50 mg of the composite material was dispersed in 80 ml of deionized water, and 20 ml of triethanolamine was dispersed in the above solution as a sacrificial agent. After continuous irradiation with a 300W xenon lamp for 5 hours, the main products of the test were CO and CH4. Figure 4 As shown in a and b, all samples showed an increase in product in proportion to irradiation time. 19 S27 Br3 and CoAl-LDH showed low CO generation. However, 66-Bi with S-type heterojunction 19 S 27 The CO production of Br3 / CoAl-LDH increased significantly within 5 hours. 19 S 27 When Br3 / CoAl-LDH was used, the highest CO production was 86.41 μmol g -1 , respectively Bi 19 S 27 Br3 and CoAl-LDH are 4 and 7 times higher. Figure 4 In b, the CH4 production of CoAl-LDH was relatively low (1.09 μmol g within 5 h of illumination). -1 ), Bi 19 S 27 Br3 did not detect CH4 generation. However, when the composite ratio was 66-Bi 19 S 27 The maximum CH4 yield in Br3 / CoAl-LDH was 3.97 μmol g -1 , which is 4 times that of CoAl-LDH.
[0049] After five cycles of experiments ( Figure 5 c) It can be seen that 66-Bi 19 S 27 The CO production of the fifth experiment of Br3 / CoAl-LDH was 95.3% of that of the first experiment, and the rate of decrease in production was relatively stable. Then, the samples were collected by centrifugation and the stability was further evaluated using XRD ( Figure 5 d) 66-Bi 19 S 27 The XRD pattern of Br3 / CoAl-LDH showed no significant changes after five consecutive runs, and the crystal structure did not change. These results confirm that 66-Bi 19 S 27 The Br3 / CoAl-LDH composite photocatalyst is reusable and relatively stable.
[0050] From the PL diagram ( Figure 6 ) can be seen that, with Bi 19 S 27 Compared with Br3 and CoAl-LDH, 66-Bi 19 S 27 The PL intensity of Br3 / CoAl-LDH is lower. Therefore, 66-Bi 19 S 27Br3 / CoAl-LDH has a stronger charge carrier separation rate and reduces the recombination rate of electrons and holes. UV-vi( Figure 7 ) shows that as Bi 19 S 27 Combination of Br3 and CoAl-LDH, 66-Bi 19 S 27 The optical absorption edge of Br3 / CoAl-LDH composites is relatively 19 S 27 The light absorption edges of Br3 and CoAl-LDH show a significant red shift. 19 S 27 Br3 / CoAl-LDH has a wider light absorption edge, which is beneficial for collecting sunlight. These results show that Bi 19 S 27 The combination of Br3 and CoAl-LDH significantly enhanced the photogenerated charge transfer and increased the light absorption capacity, thus improving the performance of photocatalytic reduction of CO2.
[0051] Figure 8 for Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 Electrochemical diagram of Br3 / CoAl-LDH. Figure 8 It can be seen that the conductivity of the composite with transient photocurrent response is higher than that of Bi 19 S 27 Conductivity of Br3 and CoAl-LDH, 66-Bi 19 S 27 The Br3 / CoAl-LDH composite showed the highest photocurrent, indicating the highest separation efficiency of charge carriers. These results are consistent with the PL test, further confirming that 66-Bi 19 S 27 Br3 / CoAl-LDH photocatalyst has a faster hole-electron separation rate. 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 The photogenerated charge transfer resistance in Br3 / CoAl-LDH composites was reported by the Nyquist circle of electrochemical impedance spectroscopy (EIS). Figure 8 d). The EIS semicircle radius of the three samples is arranged as follows: CoAl-LDH>Bi 19 S 27 Br3>66-Bi 19 S 27Br3 / CoAl-LDH. This fully demonstrates the significant reduction in charge transfer resistance due to the formation of the composite catalyst. Figure 8 e shows Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 LSV curve of Br3 / CoAl-LDH. Different initial potentials represent different CO2 reduction abilities. 19 S 27 The initial potential of Br3 / CoAl-LDH is the lowest. The lower initial potential indicates that the interfacial charge transfer between the sample and the electrode is significantly accelerated, indicating that 66-Bi 19 S 27 Br3 / CoAl-LDH vs. Bi 19 S 27 Br3 and CoAl-LDH have stronger CO2 reduction ability.
[0052] Fig. 9 for Bi 19 S 27 Br3 and CoAl-LDH (αhμ) 2 Relationship diagram with photon energy (hμ) (a, b), NiFe-LLDH (c) and Bi 19 S 27 VB XPS spectra of Br3(d), Mott-Schottky spectra of CoAl-LDH(d) and Bi5O7Br. Based on the calculation results of UV-vis DRS and Kubelka-Monk function, Bi 19 S 27 The band gap energies (Eg) of Br3 and CoAl-LDH were estimated to be 1.47 eV and 2.21 eV. Fig. 9 c and 9d show Bi 19 S 27 XPS valence band spectra of Br3 and CoAl-LDH, Bi 19 S 27 The maximum VB (EVB) of Br3 and CoAl-LDH are 0.18eV and 1.26eV, respectively. At the same time, the energy level position of the catalyst was studied by Mott-Schottky plot. 19 S 27 Br3 and CoAl-LDH are both n-type semiconductors. When a silver chloride reference electrode (SCE) is used as the reference electrode, Bi 19 S 27The flat band potentials of Br3 and CoAl-LDH are -1.29 eV and -0.95 eV, respectively. According to experience, the flat band potential position of n-type semiconductors is negative 0.20 V compared to CB. Therefore, Bi 19 S 27 The CB values of Br3 and CoAl-LDH are -1.09 V and -1.15 V (relative to SCE), respectively. The conversion equation between the saturated calomel electrode and the standard hydrogen electrode is as follows: NHE =E SCE +0.2eV, Bi 19 S 27 The CBs of Br3 and CoAl-LDH were calculated to be −1.29 and −0.95 eV, respectively.
[0053] Since the state of electrons in a substance has a great influence on its properties and functions, the properties of unpaired electrons in catalysts are detected and analyzed by ESR (electron spin resonance). Fig.10 As shown in a, Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 Br3 / CoAl-LDH·O 2- The signal is very weak, which means that no significant amount of free radicals are generated under dark conditions. However, after 5 minutes of irradiation, the 66-Bi 19 S 27 O is clearly observed in Br3 / CoAl LDH 2- Similarly, at Fig.10 In b, under dark conditions, Bi 19 S 27 Br3, CoAl-LDH and 66-Bi 19 S 27 No ·OH signal was detected in Br3 / CoAl-LDH. After 5 minutes of irradiation, 66-Bi 19 S 27 Br3 / CoAl-LDH produces a large amount of ·OH, indicating that 66-Bi 19 S 27 The Co ions in Br3 / CoAl-LDH can activate DMPO and generate free radicals. Therefore, it can be inferred that 66-Bi 19 S 27 The formation of Br3 / CoAl-LDH promoted the generation of free radicals, thereby improving the performance of photocatalytic reduction of CO2.
[0054] The embodiments are preferred implementations of the present invention, but the present invention is not limited to the above-mentioned implementations. Any obvious improvements, substitutions or modifications that can be made by those skilled in the art without departing from the essential content of the present invention belong to the protection scope of the present invention.
Claims
1. A Bi 19 S 27 Br3 / CoAl-LDH composite material, characterized in that The composite material is a rod-shaped Bi 19 S 27 Br3 fits the regular sheet structure CoAl-LDH; the Bi 19 S 27 Bi in Br3 / CoAl-LDH composites 19 S 27 The mass percentage of Br3 is 33-66%; the Bi 19 S 27 The preparation method of the Br3 / CoAl-LDH composite material comprises the following specific steps: (1) Dissolve Co(NO3)2•9H2O and Al(NO3)3•9H2O in deionized water and add Bi 19 S 27 Br3 is used to disperse it evenly to obtain a suspension; (2) Add NaOH and Na2CO3 to the suspension, stir with ultrasonic until it turns completely black, and then heat the mixture at 120-130°C for 16-17 hours; (3) After cooling to room temperature, washing and drying, Bi 19 S 27 Br3 / CoAl-LDH composite materials.
2. A Bi as claimed in claim 1 19 S 27 The preparation method of Br3 / CoAl-LDH composite material is characterized in that: The specific steps include: (1) Dissolve Co(NO3)2•9H2O and Al(NO3)3•9H2O in deionized water and add Bi 19 S 27 Br3 is used to disperse it evenly to obtain a suspension; (2) Add NaOH and Na2CO3 to the suspension, stir with ultrasonic until it turns completely black, and then heat the mixture at 120-130°C for 16-17 hours; (3) After cooling to room temperature, washing and drying, Bi 19 S 27 Br3 / CoAl-LDH composite materials.
3. Bi according to claim 2 19 S 27 The preparation method of Br3 / CoAl-LDH composite material is characterized in that: The molar ratio of Co(NO3)2•9H2O and Al(NO3)3•9H2O is 1:0.
5.
4. Bi according to claim 2 19 S 27 The preparation method of Br3 / CoAl-LDH composite material is characterized in that: Bi 19 S 27 The molar ratio of Br3 and Co(NO3)2•9H2O is 2~5:
1.
5. Bi according to claim 2 19 S 27 The preparation method of Br3 / CoAl-LDH composite material is characterized in that: The molar ratio of NaOH, Na2CO3 and Co(NO3)2•9H2O is 4:1.5:
1.
6. A Bi as claimed in claim 1 19 S 27 Application of Br3 / CoAl-LDH composite materials in photocatalytic reduction of CO2.
7. Bi according to claim 6 19 S 27 The application of Br3 / CoAl-LDH composite material in photocatalytic reduction of CO2 is characterized by: The steps include: mixing deionized water, sacrificial agent and Bi under xenon lamp irradiation 19 S 27 The Br3 / CoAl-LDH composite material was added into the photoreactor and reacted in a CO2 gas atmosphere at normal pressure.