Conductive heating glass and preparation method thereof

By coating conductive film paste on non-metallic substrates and printing silver paste, conductive heating glass is prepared, which solves the problems of uneven heating, fragility and safety of existing heating glasses, and achieves rapid and uniform heating and high light transmittance. Solution for high power usage.

CN117285259BActive Publication Date: 2024-11-05姚添辉
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311182626.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-13
Publication Date
2024-11-05
Estimated Expiration
2043-09-13

AI Technical Summary

Technical Problem

The existing heating glass has problems such as uneven heating, fragility, high voltage and large energy loss, which limits its application, and is difficult to ensure safety and hygiene.

Method used

Conductive heat-generating glass is prepared by coating conductive film slurry on a non-metallic substrate, and a solid slurry is formed by oscillating at high temperatures using mixtures of tin oxide, indium oxide, titanium oxide, zinc oxide and aluminum oxide, which are sprayed and baked until Curing, then printing silver paste on the edge to form a conductive electrode to achieve conductive heating.

Benefits of technology

It achieves uniform heating and rapid heating to 100-500℃, with a light transmittance of up to 99%. It is suitable for high-power use, with continuous high-temperature dry burning without attenuation, and has a long service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117285259B_ABST
    Figure CN117285259B_ABST
Patent Text Reader

Abstract

The present invention discloses a conductive heating glass and a preparation method thereof, and belongs to the technical field of glass plates. The method realizes the production of a conductive substrate by coating a conductive film slurry on a non-metallic substrate. The conductive heating glass prepared by the above method has uniform heating, can reach a rapid heating effect of 100-500°C in 15-20s, and the product heating process detected is stable, and the light transmittance reaches 99%; it is suitable for high-power use, the power will not decay when continuously dry-burned at high temperature, and the service life is long.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass plates, and in particular relates to a conductive heating glass and a preparation method thereof. Background Art

[0002] Glass, as a special material, is used in all aspects of work and life. Because glass has the advantages of beauty, transparency, and flatness, in addition to being used as a shield and a vehicle, people are also developing other uses for glass, such as the heating function of glass. Currently, heating glass is used in automobiles, goggles, defog windows, medical equipment, and household appliances. However, due to problems with the heating method and heating materials, the heating is uneven and fragile, high voltage is prone to safety problems, and transparency and heating cannot be well combined. These problems have always limited our expansion of the application of heating glass.

[0003] Currently, many heating devices on the market are composed of electric heating wires or electromagnetic heating. However, due to the insufficient stability and generally insufficient lifespan of the heating wires, and the excessive electromagnetic power, the resulting imaging and other problems can easily affect the user.

[0004] The heat conversion rate of the heating plate furnaces currently on the market is particularly low, which often causes a large energy loss, and safety and hygiene cannot be well guaranteed. When heating, one place is often heated while another place is not, resulting in uneven heating and poor heating effect. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing conductive heating glass, which realizes the production of conductive substrate by coating a conductive film slurry on a non-metallic substrate. The conductive heating glass prepared by the above method has uniform heating and can reach a rapid heating effect of 100-500°C in 15-20s. Moreover, the product heating process is stable and the light transmittance reaches 99%; it is suitable for high-power use, and the power will not decay during continuous high-temperature dry burning, and the service life is long.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing conductive heating glass comprises the following steps:

[0008] S1. Preparation of conductive film slurry:

[0009] Select tin oxide, indium oxide, titanium oxide, zinc oxide and aluminum oxide, mix them, add pure water and mix them evenly into a solid slurry, and oscillate and mix the solid slurry under heating conditions to obtain a conductive film slurry;

[0010] S2. Preparation of conductive glass:

[0011] Spraying the conductive film slurry in S1 onto the surface of the non-metallic substrate after the heating treatment, baking until the conductive film slurry is solidified on the non-metallic substrate, and cooling to room temperature;

[0012] S3. Preparation of conductive electrodes:

[0013] Silver paste is printed on the edge of the conductive glass, and heated and baked until the silver paste is fixed on the conductive glass to obtain conductive heating glass.

[0014] Preferably, in S1, each raw material is selected according to the following mass fractions:

[0015] 38-114 parts of tin oxide, 7-21 parts of indium oxide, 2-6 parts of titanium oxide, 1-6 parts of zinc oxide and 1-4 parts of aluminum oxide.

[0016] Preferably, in S1, each raw material is selected according to the following mass fractions:

[0017] 76 parts of tin oxide, 15 parts of indium oxide, 4 parts of titanium oxide, 3 parts of zinc oxide and 2 parts of aluminum oxide.

[0018] The purpose of the above-mentioned raw materials is to prepare a conductive raw material after mixing all the raw materials, and then attach it to the microcrystalline glass at high temperature to generate current and generate heat.

[0019] Preferably, in S1, the solid content of the raw materials in the solid-containing slurry is 80wt%-85wt%.

[0020] Preferably, in S1, the temperature of the heating condition is not less than 300°C.

[0021] Preferably, in S2, the heating temperature of the non-metallic substrate after the heating treatment is not less than 700° C.; the heating time is 100-120 seconds;

[0022] The non-metal substrate is a microcrystalline glass substrate or a quartz glass substrate.

[0023] Preferably, in S2, the baking temperature is not less than 700° C., and the baking time is 50-60 seconds.

[0024] Preferably, in S3, the heating and baking temperature is 350-380° C., and the duration is 3-8 seconds.

[0025] A conductive heating glass is obtained by the preparation method.

[0026] The conductive heating glass can be used in the preparation of heating household appliances and industrial heating products.

[0027] Compared with the prior art, the present invention has at least the following technical effects:

[0028] The present invention provides a method for preparing conductive heating glass, which is achieved by coating a conductive film slurry on a non-metallic substrate to produce a conductive substrate. The conductive heating glass prepared by the above method has uniform heating and can reach a rapid heating effect of 100-500°C in 15-20s. Moreover, the product heating process is stable and the light transmittance reaches 99%; it is suitable for high-power use, and the power will not decay during continuous high-temperature dry burning, and has a long service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic diagram of the test sample prepared in Example 3;

[0030] Figure 2 This is a schematic diagram of the temperature curve monitored during the test. DETAILED DESCRIPTION

[0031] The embodiments of the present invention will be described in detail below in conjunction with examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0032] Embodiment 1:

[0033] Each raw material is selected according to the following mass fractions:

[0034] 380 grams of tin oxide, 70 grams of indium oxide, 20 grams of titanium oxide, 10 grams of zinc oxide and 10 grams of aluminum oxide.

[0035] A method for preparing conductive heating glass comprises the following steps:

[0036] S1. Preparation of conductive film slurry:

[0037] Select tin oxide, indium oxide, titanium oxide, zinc oxide and aluminum oxide, mix them, add pure water and mix them evenly into a solid slurry with a solid content of 80wt%, and oscillate and mix the solid slurry evenly under a heating temperature of not less than 300° C. to obtain a conductive film slurry;

[0038] S2. Preparation of conductive glass:

[0039] Spray the conductive film slurry in S1 onto the surface of the microcrystalline glass substrate that has been heated to no less than 700° C., bake at a temperature no less than 700° C., bake for 50 seconds until the conductive film slurry is solidified on the microcrystalline glass substrate, and cool to room temperature;

[0040] S3. Preparation of conductive electrodes:

[0041] Print silver paste on the edge of the conductive glass, heat the temperature to 350-380°C, and bake for 3-8s until the silver paste is fixed on the conductive glass to obtain conductive heating glass.

[0042] Embodiment 2:

[0043] Each raw material is selected according to the following mass fractions:

[0044] 1140 grams of tin oxide, 210 grams of indium oxide, 60 grams of titanium oxide, 60 grams of zinc oxide and 40 grams of aluminum oxide.

[0045] A method for preparing conductive heating glass comprises the following steps:

[0046] S1. Preparation of conductive film slurry:

[0047] Select tin oxide, indium oxide, titanium oxide, zinc oxide and aluminum oxide, mix them, add pure water and mix them evenly into a solid slurry with a solid content of 85wt%, and oscillate and mix the solid slurry evenly under a heating temperature of not less than 300° C. to obtain a conductive film slurry;

[0048] S2. Preparation of conductive glass:

[0049] Spray the conductive film slurry in S1 onto the surface of the non-metallic substrate heated to not less than 700°C, bake at a temperature not less than 700°C, bake for 60 seconds until the conductive film slurry is solidified on the non-metallic substrate, and cool to room temperature;

[0050] S3. Preparation of conductive electrodes:

[0051] Print silver paste on the edge of the conductive glass, heat the temperature to 350-380°C, and bake for 3-8s until the silver paste is fixed on the conductive glass to obtain conductive heating glass.

[0052] Embodiment 3:

[0053] Each raw material is selected according to the following mass fractions:

[0054] 760 grams of tin oxide, 150 grams of indium oxide, 40 grams of titanium oxide, 30 grams of zinc oxide and 20 grams of aluminum oxide.

[0055] A method for preparing conductive heating glass comprises the following steps:

[0056] S1. Preparation of conductive film slurry:

[0057] Select tin oxide, indium oxide, titanium oxide, zinc oxide and aluminum oxide, mix them, add pure water and mix them evenly into a solid slurry with a solid content of 80wt%, and oscillate and mix the solid slurry evenly under a heating temperature of not less than 300° C. to obtain a conductive film slurry;

[0058] S2. Preparation of conductive glass:

[0059] Spray the conductive film slurry in S1 onto the surface of the microcrystalline glass substrate that has been heated to no less than 700° C., bake at a temperature no less than 700° C., bake for 50 seconds until the conductive film slurry is solidified on the microcrystalline glass substrate, and cool to room temperature;

[0060] S3. Preparation of conductive electrodes:

[0061] Print silver paste on the edge of the conductive glass, heat the temperature to 350-380°C, and bake for 3-8s until the silver paste is fixed on the conductive glass to obtain conductive heating glass.

[0062] Inspection Report:

[0063] Report number: 20210703W18073

[0064] Sample: As Figure 1 Shown

[0065] Electric crystal furnace, product model: QLWJ-22 / 16A Rated power: 1600W Rated voltage: 220V

[0066] Rated frequency: 50Hz

[0067] Test instructions:

[0068] 1. Rated value: Rated voltage or voltage range: 220V

[0069] Rated current or current range: / ; Rated power or power range: 2200W, 2100W; Rated frequency or frequency range: 50Hz; Rated capacity (or volume): /

[0070] 2. Power supply nature: single-phase AC;

[0071] 3. Anti-electric shock protection category: Class I, Class II;

[0072] 4. Protection level: IP

[0073] 5. Equipment type: portable

[0074] 6. Working mode: continuous working

[0075] 7. Equipment control method: electronic control

[0076] 8. Power cord plug type: single-phase two-pole, single-phase three-pole

[0077] 9. Connection method to the power supply: A power cord with a plug

[0078]

[0079] like Figure 2 As shown, it is a schematic diagram of the temperature curve monitored during the test, which is used to verify the heating performance. Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a conductive heating glass, characterized in that: The steps include: S1. Preparation of conductive film slurry: Tin oxide, indium oxide, titanium oxide, zinc oxide and aluminum oxide are selected and mixed, and purified water is added to mix to form a solid slurry. The solid slurry is oscillated and mixed under heating conditions to obtain a conductive film slurry; the raw materials are selected according to the following mass fractions: 38-114 parts of tin oxide, 7-21 parts of indium oxide, 2-6 parts of titanium oxide, 1-6 parts of zinc oxide and 1-4 parts of aluminum oxide; The solid content of the raw material in the solid-containing slurry is 80wt%-85wt%; The temperature of the heating condition is not less than 300°C; S2. Preparation of conductive glass: Spraying the conductive film slurry in S1 onto the surface of the non-metallic substrate after the heating treatment, baking until the conductive film slurry is solidified on the non-metallic substrate, and cooling to room temperature; The baking temperature is not less than 700°C, and the baking time is 50-60s; S3. Preparation of conductive electrodes: Printing silver paste at the edge of the conductive glass, heating and baking until the silver paste is fixed on the conductive glass, thereby obtaining conductive heating glass; The heating and baking temperature is 350-380° C., and the duration is 3-8 seconds.

2. A conductive heating glass, characterized in that: Obtained by the preparation method described in claim 1.