Environmentally friendly degradable plastic and preparation method thereof

By using carbon nanotubes and modified zinc oxide in polylactic acid films, the mechanical and antibacterial properties of the film are significantly improved, the lack of performance in the prior art is solved, and efficient plastic film preparation is achieved.

CN117285734BActive Publication Date: 2024-11-19SHENZHEN JUYI FII CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311334500.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-16
Publication Date
2024-11-19
Estimated Expiration
2043-10-16

AI Technical Summary

Technical Problem

The prior art has shortcomings in improving the mechanical properties and antibacterial properties of polylactic acid antibacterial membranes, and it is difficult to significantly improve the performance in both aspects.

Method used

Carbon nanotubes are used as hard template agent to prepare hydrotalcite, and modified by quaternary ammonium salt, combined with xylan coated with modified zinc oxide, and ultrasonic dispersed with polylactic acid to form an improved plastic film, which is improved by this method. Mechanical properties and antibacterial properties of the membrane.

Benefits of technology

The mechanical properties and antibacterial properties of polylactic acid film are significantly improved, making it have good mechanical properties and antibacterial properties, and at the same time, the process is simple, the raw materials are rich and the cost is low.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of plastic films, and specifically relates to an environmentally friendly degradable plastic and a preparation method thereof. Hydrotalcite-like materials are prepared by using carbon nanotubes as hard templates, and then modified by quaternary ammonium salts to obtain product A, and product B is obtained by coating silver-modified zinc oxide with xylan, and product A, product B and polylactic acid are ultrasonically dispersed in dichloromethane, ultrasonically treated, and then stirred to obtain a mixture, and then the mixture is coated, and the plastic film is obtained after the dichloromethane is completely volatilized. The mechanical properties and antibacterial properties of the polylactic acid film are improved by the combination of product A and product B, so that the film has good mechanical properties and antibacterial properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of plastic technology, and more specifically, relates to an environmentally friendly degradable plastic and a preparation method thereof. Background Art

[0002] Polylactic acid (PLA) is easy to obtain and can be made from agricultural products such as starch. Its good biocompatibility and biodegradability are increasingly valued by people, and PLA's excellent mechanical properties allow it to be processed into films in a variety of ways. PLA is a crystalline polymer material with certain antibacterial properties, and will form carbon dioxide and water after biodegradation.

[0003] CN111333888A discloses a degradable polylactic acid antibacterial film and a preparation method thereof. The method comprises: mixing nano titanium dioxide with water to obtain a first solution; heating the first mixture to about 80 to 160°C, wherein the first mixture is selected from polylactic acid, ethylene vinyl acetate copolymer (EVA), an opening lubricant masterbatch, an additive or a mixture thereof; adding the first solution to the heated first mixture at about 80 to 160°C to obtain a second mixture; and subjecting the second mixture to single-layer or multi-layer co-extrusion, film blowing or casting to obtain the degradable polylactic acid antibacterial film. The degradable polylactic acid antibacterial film disclosed in the present invention has antibacterial and degradable functions.

[0004] CN113817205A discloses a photocatalytic polylactic acid antibacterial film and a preparation method and application thereof. The present invention utilizes low-temperature plasma technology to modify the surface of polylactic acid material so that a large number of active carboxyl groups are generated on its surface. On this basis, the carboxyl groups on the surface of the polylactic acid film are innovatively covalently reacted with a photosensitizer, and combined with blue LED light irradiation, a photocatalytic PLA antibacterial film is prepared; the present invention organically integrates and innovates photodynamic technology, low-temperature plasma technology and food packaging materials to develop packaging film materials with efficient sterilization function, which is a breakthrough in the food packaging industry and also provides new theoretical ideas and innovative practices for the future development of functional food packaging film materials; the antibacterial film of the present invention is a food packaging material that can kill common pathogenic bacteria and spoilage bacteria in food in a green and efficient manner, and further uses these new packaging films to package salmon and other foods, greatly extending the shelf life of the food.

[0005] CN113667168A discloses a method for preparing a degradable antibacterial packaging film with antibacterial and water-blocking properties. A composite antibacterial agent is prepared by mixing nano zinc oxide with other antibacterial agents, and the composite antibacterial agent is dispersed in a mixture of polylactic acid and polyadipate / butylene terephthalate to enhance the antibacterial properties of the film. At the same time, a coating method is used to coat the modified polyvinyl alcohol on the composite film to enhance the water-blocking property of the material. The composite film has a good antibacterial and fresh-keeping effect and is suitable for fresh food packaging. In addition, the method complies with the principle of "green packaging" and is conducive to the sustainable development of the ecology.

[0006] CN113004568A discloses a composite antibacterial food packaging film and its preparation method. Its preparation route is "casting film sulfonation ion exchange in-situ reduction": polylactic acid is used as film-forming material, chitosan is used as natural antibacterial agent, ethyl acetate is used as organic solvent to prepare casting slurry and chitosan polylactic acid blended base film is prepared by casting method, then reacted with sulfonating agent to prepare sulfonated film, and further exchanged with metal ions with excellent antibacterial activity such as silver ions and copper ions to prepare ion-based film, and on this basis, a single substance nano-based antibacterial food packaging film is prepared by in-situ reduction reaction. The antibacterial film prepared by the present invention combines the advantages of natural antibacterial agents and inorganic metal antibacterial agents, solves the disadvantage of weak antibacterial performance of natural antibacterial agents, and thus makes the antibacterial performance of the film stronger.

[0007] From the above content, it can be seen that the antibacterial properties of plastics can be improved by adding organic antibacterial agents or inorganic antibacterial agents to the film raw materials, but there are still deficiencies in having excellent mechanical properties and antibacterial properties. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art, and provide an environmentally friendly degradable plastic and a preparation method thereof. Hydrotalcite-like materials are prepared by using carbon nanotubes as hard templates, and then modified by quaternary ammonium salts to obtain product A, and product B is obtained by coating silver-modified zinc oxide with xylan, and product A, product B and polylactic acid are ultrasonically dispersed in dichloromethane, ultrasonically treated, and then stirred to obtain a mixture, and then the mixture is coated, and the dichloromethane is volatilized to obtain the plastic film. The mechanical properties and antibacterial properties of the polylactic acid film are improved by the combination of product A and product B, so that the film has good mechanical properties and antibacterial properties.

[0009] The purpose of the invention is to provide a method for preparing environmentally friendly degradable plastics.

[0010] Another object of the present invention is to provide an environmentally friendly and degradable plastic.

[0011] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0012] A method for preparing an environmentally friendly and degradable plastic, the method comprising the following steps:

[0013] (1) Ultrasonic dispersion of magnesium salt, zinc salt, copper salt, chromium salt and carbon nanotubes in deionized water to obtain a dispersion; then urea is added to the dispersion, stirred evenly, and then heated to 110-130° C. for reaction for 14-18 hours to obtain product a, product a is calcined to obtain product b, product b and didecyl dimethyl ammonium chloride are dispersed in deionized water; then stirred at 60-80° C. for 2-4 hours, filtered, and vacuum dried to obtain product A;

[0014] (2) ultrasonically dispersing xylan, silver nitrate and zinc nitrate in deionized water, ultrasonically, then raising the temperature to 40-60°C and stirring for 5-7 hours; then dropping sodium hydroxide solution into the mixed solution to adjust the pH of the mixed solution to 11; then continuing to stir; standing, centrifuging, washing with deionized water 3 times, and vacuum drying to obtain product B;

[0015] (3) Ultrasonic dispersion of product A, product B and polylactic acid in dichloromethane, ultrasonic treatment, stirring to obtain a mixture, and then coating the mixture, and after the dichloromethane is completely evaporated, the plastic film is obtained.

[0016] According to a further technical solution, in step (1), the magnesium salt is at least one of magnesium nitrate, magnesium chloride and magnesium acetate; the zinc salt is at least one of zinc nitrate, zinc chloride and zinc acetate; the copper salt is at least one of copper nitrate, copper chloride and copper acetate; and the chromium salt is at least one of chromium nitrate, chromium chloride and chromium acetate.

[0017] A further preferred technical solution is that in step (1), the ratio of the magnesium salt, zinc salt, copper salt, chromium salt, carbon nanotubes and urea is: 10mmol: 0.4-0.8mmol: 0.3-0.5mmol: 25-35mmol: 10g: 50-70mmol; the mass ratio of the product b and didecyldimethylammonium chloride is 10: 0.02-0.06.

[0018] According to a further technical solution, in step (1), the calcination is performed at 500-600° C. for 8-12 hours; and the vacuum drying is performed at 60-80° C. for 10-14 hours.

[0019] According to a further technical solution, in step (2), the mass ratio of xylan, silver nitrate and zinc nitrate is 1:0.02-0.06:0.7-0.9.

[0020] According to a further preferred technical solution, in step (2), the ultrasonication time is 30 to 50 minutes; the continued stirring time is 20 to 40 minutes; and the standing time is 4 to 8 hours.

[0021] In a further preferred technical solution, in step (2), the vacuum drying is performed at 50-70° C. for 10-14 h; and the concentration of the sodium hydroxide solution is 1 mol / L.

[0022] Preferably, in step (3), the ultrasonic treatment time is 30 to 50 minutes; and the stirring time is 3 to 5 hours.

[0023] According to a further preferred embodiment, in step (3), the mass ratio of the product A, the product B and the polylactic acid is 1-3:2-4:100.

[0024] An environmentally friendly and degradable plastic is prepared based on the above-mentioned method for preparing an environmentally friendly and degradable plastic.

[0025] The present invention has the following beneficial effects:

[0026] (1) The hydrotalcite-like material prepared by using carbon nanotubes as a hard template can significantly improve the specific surface area of ​​the hydrotalcite-like material and enhance its activity. At the same time, the antibacterial property can be significantly improved by modification with didecyl dimethyl ammonium chloride.

[0027] (2) The antibacterial material is obtained by coating silver-modified zinc oxide with xylan, and the combination of the remaining quaternary ammonium salt-modified hydrotalcite can significantly improve the antibacterial and mechanical properties of the film.

[0028] (3) The raw material sources of the present invention are abundant, the preparation process is simple and the cost is low. DETAILED DESCRIPTION

[0029] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0030] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0031] Example 1

[0032] A method for preparing an environmentally friendly and degradable plastic, the method comprising the following steps:

[0033] (1) 10 mmol magnesium nitrate, 0.6 mmol zinc chloride, 0.4 mmol copper acetate, 30 mmol chromium nitrate and 10 g carbon nanotubes were ultrasonically dispersed in 100 mL deionized water to obtain a dispersion; 60 mmol urea was then added to the dispersion, stirred evenly, and then heated to 120° C. for reaction for 16 h to obtain product a, and product a was calcined at 550° C. for 10 h to obtain product b, and 10 g product b and 0.04 g didecyl dimethyl ammonium chloride were dispersed in 100 mL deionized water; then stirred at 70° C. for 3 h, filtered, and vacuum dried at 70° C. for 12 h to obtain product A;

[0034] (2) 10 g of xylan, 0.4 g of silver nitrate and 8 g of zinc nitrate were ultrasonically dispersed in 100 mL of deionized water for 50 min, and then the temperature was raised to 50°C and stirred for 6 h; then a 1 mol / L sodium hydroxide solution was added dropwise to the mixed solution to adjust the pH of the mixed solution to 11; then stirring was continued for 40 min; the mixture was allowed to stand for 6 h, centrifuged, washed with deionized water 3 times, and vacuum dried at 60°C for 12 h to obtain product B;

[0035] (3) 2 g of product A, 3 g of product B and 100 g of polylactic acid are ultrasonically dispersed in 220 g of dichloromethane, ultrasonically treated for 40 min, and then stirred for 4 h to obtain a mixture, and then the mixture is coated, and after the dichloromethane is completely evaporated, the plastic film is obtained.

[0036] Example 2

[0037] A method for preparing an environmentally friendly and degradable plastic, the method comprising the following steps:

[0038] (1) 10 mmol of magnesium chloride, 0.8 mmol of zinc acetate, 0.3 mmol of copper nitrate, 35 mmol of chromium chloride and 10 g of carbon nanotubes were ultrasonically dispersed in 100 mL of deionized water to obtain a dispersion; 70 mmol of urea was then added to the dispersion, stirred evenly, and then heated to 130° C. for reaction for 14 h to obtain product a, and product a was calcined at 600° C. for 8 h to obtain product b, and 10 g of product b and 0.06 g of didecyl dimethyl ammonium chloride were dispersed in 100 mL of deionized water; then stirred at 80° C. for 2 h, filtered, and vacuum dried at 80° C. for 10 h to obtain product A;

[0039] (2) 10 g of xylan, 0.6 g of silver nitrate and 7 g of zinc nitrate were ultrasonically dispersed in 100 mL of deionized water for 50 min, and then the temperature was raised to 60°C and stirred for 5 h; then a 1 mol / L sodium hydroxide solution was added dropwise to the mixed solution to adjust the pH of the mixed solution to 11; then stirring was continued for 40 min; the mixture was allowed to stand for 4 h, centrifuged, washed with deionized water 3 times, and vacuum dried at 70°C for 10 h to obtain product B;

[0040] (3) 3 g of product A, 2 g of product B and 100 g of polylactic acid are ultrasonically dispersed in 220 g of dichloromethane, ultrasonically treated for 50 min, and then stirred for 3 h to obtain a mixture, and then the mixture is coated, and after the dichloromethane is completely evaporated, the plastic film is obtained.

[0041] Example 3

[0042] A method for preparing an environmentally friendly and degradable plastic, the method comprising the following steps:

[0043] (1) 10 mmol of magnesium acetate, 0.4 mmol of zinc nitrate, 0.5 mmol of copper chloride, 25 mmol of chromium acetate and 10 g of carbon nanotubes were ultrasonically dispersed in 100 mL of deionized water to obtain a dispersion; 50 mmol of urea was then added to the dispersion, stirred evenly, and then heated to 110° C. for reaction for 18 h to obtain product a, and product a was calcined at 500° C. for 12 h to obtain product b, and 10 g of product b and 0.02 g of didecyl dimethyl ammonium chloride were dispersed in 100 mL of deionized water; then stirred at 60° C. for 4 h, filtered, and vacuum dried at 60° C. for 14 h to obtain product A;

[0044] (2) 10 g of xylan, 0.2 g of silver nitrate and 9 g of zinc nitrate were ultrasonically dispersed in 100 mL of deionized water for 30 min, and then the temperature was raised to 40°C and stirred for 7 h; then a 1 mol / L sodium hydroxide solution was added dropwise to the mixed solution to adjust the pH of the mixed solution to 11; then stirring was continued for 20 min; the mixture was allowed to stand for 8 h, centrifuged, washed with deionized water 3 times, and vacuum dried at 50°C for 14 h to obtain product B;

[0045] (3) 1 g of product A, 4 g of product B and 100 g of polylactic acid are ultrasonically dispersed in 220 g of dichloromethane, ultrasonically treated for 30 min, and then stirred for 5 h to obtain a mixture, and then the mixture is coated, and after the dichloromethane is completely evaporated, the plastic film is obtained.

[0046] Comparative Example 1

[0047] The steps and conditions are the same as those in Example 1 except that 5 g of product B is used to replace 2 g of product A and 3 g of product B.

[0048] Comparative Example 2

[0049] Except for the difference, the steps and conditions are the same as those of Example 1, except that 1 mmol of zinc chloride is used to replace 0.6 mmol of zinc chloride and 0.4 mmol of copper acetate.

[0050] Comparative Example 3

[0051] Except for the difference, the steps and conditions are the same as those of Example 1, except that 10 mmol of magnesium nitrate, 0.6 mmol of zinc chloride and 0.4 mmol of copper acetate are replaced by 11 mmol of magnesium nitrate.

[0052] Comparative Example 4

[0053] The steps and conditions are the same as those of Example 1 except that 8.4 g of zinc nitrate is used to replace 0.4 g of silver nitrate and 8 g of zinc nitrate.

[0054] The mechanical properties of Example 1 and Control Example 4 were tested according to GB / T 1040-2006. See 1 for specific test results.

[0055] Table 1:

[0056] Example 1 Comparative Example 4 Tensile strength(MPa) 68.4 53.4

[0057] The antibacterial properties of Examples 1-3 and Comparative Examples 1-4 were tested according to QB / T 2591-2003. The specific test results are shown in Table 2:

[0058] Table 2

[0059] Escherichia coli antibacterial rate (%) Antibacterial rate of Staphylococcus aureus (%) Example 1 99.8 99.4 Example 2 99.6 99.1 Example 3 99.2 98.7 Comparative Example 1 98.1 97.6 Comparative Example 2 95.3 94.7 Comparative Example 3 97.6 97.2 Comparative Example 4 93.6 92.7

[0060] It can be seen from Table 1 and Table 2 that the environmentally friendly degradable plastic prepared by the present invention has excellent mechanical properties and antibacterial properties by utilizing the interaction between components.

[0061] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing environmentally friendly and degradable plastics, Features: The preparation method comprises the following steps: (1) Ultrasonic dispersion of magnesium salt, zinc salt, copper salt, chromium salt and carbon nanotubes in deionized water to obtain a dispersion; then adding urea to the dispersion, stirring evenly, and then heating to 110-130° C. to react for 14-18 hours to obtain product a, calcining product a to obtain product b, and dispersing product b and didecyl dimethyl ammonium chloride in deionized water; then stirring at 60-80° C. for 2-4 hours, filtering, and vacuum drying to obtain product A; (2) Ultrasonic dispersion of xylan, silver nitrate and zinc nitrate in deionized water, ultrasonication, and then heating to 40-60°C and stirring for 5-7 hours; then dropwise adding sodium hydroxide solution to the mixed solution to adjust the pH of the mixed solution to 11; then continue stirring; let stand, centrifuge, wash with deionized water 3 times, and vacuum dry to obtain product B; (3) ultrasonically dispersing the product A, the product B and the polylactic acid in dichloromethane, ultrasonically treating, and then stirring to obtain a mixture, and then coating the mixture, and after the dichloromethane is completely volatilized, obtaining the plastic film; In step (1), the ratio of the magnesium salt, zinc salt, copper salt, chromium salt, carbon nanotubes and urea is: 10mmol: 0.4~0.8mmol: 0.3~0.5mmol: 25~35mmol: 10g: 50~70mmol; the mass ratio of the product b and didecyldimethylammonium chloride is 10: 0.02~0.06; in step (2), the mass ratio of xylan, silver nitrate and zinc nitrate is 1: 0.02~0.06: 0.7~0.9; in step (3), the mass ratio of the product A, product B and polylactic acid is 1~3: 2~4:

100.

2. A method for preparing an environmentally friendly and degradable plastic according to claim 1, Features: In step (1), the magnesium salt is at least one of magnesium nitrate, magnesium chloride, and magnesium acetate; the zinc salt is at least one of zinc nitrate, zinc chloride, and zinc acetate; the copper salt is at least one of copper nitrate, copper chloride, and copper acetate; and the chromium salt is at least one of chromium nitrate, chromium chloride, and chromium acetate.

3. A method for preparing an environmentally friendly and degradable plastic according to claim 1, Features: In step (1), the calcination is performed at 500-600° C. for 8-12 hours; and the vacuum drying is performed at 60-80° C. for 10-14 hours.

4. A method for preparing an environmentally friendly and degradable plastic according to claim 1, Features: In step (2), the ultrasonication time is 30 to 50 minutes; the continued stirring time is 20 to 40 minutes; and the standing time is 4 to 8 hours.

5. A method for preparing an environmentally friendly and degradable plastic according to claim 1, Features: In step (2), the vacuum drying is performed at 50-70° C. for 10-14 hours; and the concentration of the sodium hydroxide solution is 1 mol / L.

6. A method for preparing an environmentally friendly and degradable plastic according to claim 1, Features: In step (3), the ultrasonic treatment time is 30 to 50 minutes; the stirring time is 3 to 5 hours.

7. An environmentally friendly degradable plastic prepared according to the method for preparing an environmentally friendly degradable plastic according to any one of claims 1 to 6.