A low-cost lithium extraction process without roasting of high-calcium clay-type lithium ore
Through a roasting-free low-cost process, chemical dissociation and strong acid leaching technology are used to destroy the calcite-wrapped structure in high-calcium clay-type lithium ores, achieve effective extraction of lithium chlorite, and solve the energy consumption in traditional lithium ore metallurgical processes. The problem of high efficiency and high cost has improved the extraction efficiency and resource utilization of lithium.
Patent Information
- Application Number
- CN202311266972.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-09-28
AI Technical Summary
In the traditional lithium ore metallurgical process, the roasting process of high-calcium clay-type lithium ores consumes high energy, is expensive, and pollutes the environment. It is difficult to effectively extract lithium elements from high-calcium clay-type lithium ores using existing technology.
Using a low-cost process that does not require roasting, it is directly filtered without washing after grinding and chemical dissociation, followed by strong acid leaching, using hydrochloric acid or nitric acid to react with minerals to destroy the structure of calcite wrapping lithium chlorite and promote the dissociation and dissociation of lithium ions. Leaching.
It greatly reduces production and investment energy consumption, shortens the metallurgical process, improves lithium extraction efficiency, reduces the amount of leaching slag and gypsum production, and reduces development and utilization costs.
Smart Images

Figure CN117344153B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical metallurgy, and specifically relates to a low-cost lithium extraction process for high-calcium clay-type lithium ore without roasting. Background Art
[0002] Lithium mineral resources are a strategic resource with a wide range of applications. Due to the rapid development of new energy fields, the demand for lithium salts has increased sharply. Traditional lithium mineral resources cannot meet the supply of lithium, and new lithium mineral resources are urgently needed to be developed and utilized. Although clay-type lithium ore has a low lithium grade, it has large reserves. If it can be developed using appropriate methods, it will be a very promising source of lithium demand.
[0003] At present, the lithium resources used in industry are mainly spodumene ore, lithium mica ore and salt lake brine. my country's self-supply of the above lithium resources is insufficient, and its external dependence is as high as 60%. Therefore, finding new types of lithium resources with economic value has become an urgent task for my country's current geological exploration. Now a rare medium-large lithium resource prospecting area has been discovered in Liuzhi Pingqiao, Guizhou Province. The lithium oxide reserves (average grade: 0.4%) are preliminarily estimated to exceed 40,000 tons, of which lithium is mainly present in the form of lithium chlorite and distributed in calcite veins (Ye Lin, Xiang Zhenzhong, Wu Tao, etc. The discovery and significance of hydrothermal lithium chlorite of lithium resources in Liuzhi Pingqiao, Guizhou. Acta Mineralogica Sinica: 1-2 [2023-07-29]). Literature reports that the minerals of sedimentary lithium mines in Liuzhi, Guizhou are mainly lithium chlorite (21.10%), quartz (18.48%), calcite (19.10%), pyrite (5.86%) and other minerals. Since lithium chlorite is fine in particle size and its crystal size is generally less than 0.20-0.01 mm, it is difficult to achieve lithium enrichment and recovery using traditional mineral processing methods. Only metallurgical methods can be used to enrich and recover lithium in the clay-type lithium ore (Hui Bo, Gong Daxing, Chen Wei. Study on the occurrence state of lithium in sedimentary lithium ores in Liuzhi, Guizhou [J]. Nonferrous Metals (Mineral Processing Part), 2021, 47(11): 1-4). However, in this type of clay-type lithium ore, the calcite veins wrap around the lithium chlorite, which will hinder the enrichment and recovery of lithium elements. Therefore, it is necessary to use metallurgical methods to destroy the mineral structure and release the lithium chlorite.
[0004] At present, there are no reports on methods specifically for extracting lithium from high-calcium clay-type lithium ores. Only a few literatures and patents report on methods for extracting lithium from low-grade lithium-containing clay ores. From the existing literature and patents, for clay-type lithium ores where lithium mainly exists in the form of minerals or isomorphous forms, most of them are treated by "blank roasting-sulfuric acid leaching" or "composite additive roasting-leaching" processes. For example, CN116240399A, a method for selectively leaching lithium from clay-type lithium ore, discloses a process of roasting + leaching with water-soluble fluoride salt; CN116397108A, a method for extracting lithium from lithium-containing ore, discloses a process of roasting + organic acid leaching; CN114368764A, a method for directly preparing lithium sulfate from hard rock lithium ore, discloses a process of roasting with sulfate additive; CN116179874A, a method for separating and extracting lithium from carbonate clay-type lithium ore, discloses a process of sulfuric acid leaching + precipitation with precipitant + roasting; the invention patent "A method for extracting lithium ions from clay-type lithium ore with extremely low lithium grade using ion replacement" (application publication number CN115976337A) discloses a process of sodium salt roasting; CN116065037A, a method for leaching lithium from clay-type lithium ore using recyclable solid acid, discloses a process of roasting + oxalic acid leaching.
[0005] It is not difficult to see from the above process that roasting is one of the necessary steps to process clay-type lithium ores where lithium exists in the form of independent minerals or isomorphous forms. This is because the mineral structure of low-grade clay-type lithium resources is complex, and lithium-containing minerals are often wrapped or intermixed with clay minerals and other minerals, and roasting is required to destroy the structure of clay minerals and other minerals. Although the roasting process can bring a good leaching rate for leaching, there are obvious disadvantages. For example, roasting requires a lot of heat energy and has relatively high requirements for equipment. During roasting, elements such as S in the ore will also volatilize, and additional equipment is required to treat the exhaust gas, resulting in increased production costs.
[0006] In summary, the extraction of lithium from clay-type lithium ore currently mostly requires roasting, but roasting requires high temperature, high energy consumption, and high production cost. Moreover, there is no efficient utilization method for complex high-calcium clay-type lithium ore (Li2O content is less than 1%, CaO content is 10%-30%). Therefore, the development of a comprehensive utilization process for high-calcium clay-type lithium ore without roasting is of great significance to promote the transformation of geological scientific and technological achievements and the development of the lithium industry chain. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a low-cost lithium extraction process from high-calcium clay-type lithium ore without roasting, which destroys the structure of calcite encapsulating lithium chlorite and can separate the lithium chlorite without roasting, greatly shortening the existing lithium ore metallurgical process and significantly reducing the energy consumption and cost required for production and investment.
[0008] The object of the present invention is achieved through the following technical scheme: a process for extracting lithium from high-calcium clay-type lithium ore without roasting and at low cost, which comprises the following steps:
[0009] S1. Grinding: Grinding high calcium clay-type lithium ore to -0.074 mm, accounting for 60%-90%; preferably grinding to -0.074 mm, accounting for 75%-85%;
[0010] The high calcium clay-type lithium ore has a Li2O content of less than 1% and a CaO content of 10%-30%, and CaO mainly exists in the form of calcite;
[0011] S2, chemical dissociation: adding the ground high-calcium clay-type lithium ore to hydrochloric acid or nitric acid for chemical dissociation, and filtering directly without washing after the chemical dissociation to obtain wet dissociation slag and dissociation liquid;
[0012] Wherein, the concentration of the hydrochloric acid or nitric acid is 2-8 mol / L, and the liquid-solid ratio of chemical dissociation is 3-9 L / kg; preferably, the concentration of the hydrochloric acid or nitric acid is 3-6 mol / L, and the liquid-solid ratio of chemical dissociation is 4-6 L / kg;
[0013] The non-washing filtration refers to filtering the wet dissociation residue without washing with water, so that part of the chloride or nitrate and residual acid are retained in the wet dissociation residue; the chloride or nitrate content in the wet dissociation residue is 2.5-5%, and the residual acid content is 1-3%;
[0014] S3, strong acid leaching: the wet dissociation residue is directly subjected to strong acid leaching with sulfuric acid while hot, and the lithium-rich leaching solution and aluminum-silicon leaching residue are obtained by filtration;
[0015] Wherein, the concentration of sulfuric acid is 2-6 mol / L, and the liquid-solid ratio of strong acid leaching is 3-7 L / kg; preferably, the concentration of sulfuric acid solution is 3-5 mol / L, and the liquid-solid ratio of strong acid leaching is 4-6 L / kg.
[0016] Furthermore, in step S2, the temperature of the chemical dissociation is 30°C-90°C, and the time is 2-6 hours; preferably, the temperature of the chemical dissociation is 50°C-80°C, and the time is 3-5 hours.
[0017] Furthermore, in step S2, the dissociation liquid is used as a high-calcium clay-type lithium ore after mixed grinding with hydrochloric acid or nitric acid for preliminary dissociation, and preliminary dissociation slag and preliminary dissociation liquid are obtained after preliminary dissociation and filtration, and the preliminary dissociation liquid slag can be used as a raw material for chemical dissociation. The preliminary dissociation liquid can be recycled again.
[0018] Preferably, in step S2, the chloride or nitrate content in the wet dissociation residue without washing and filtering is 3-4.5%, and the residual acid content is 1.5-2.5%;
[0019] Furthermore, in step S3, the temperature of the strong acid leaching is 80°C-120°C, and the time is 1.5-6h; preferably, the temperature of the strong acid leaching is 90°C-105°C, and the time is 3-5h;
[0020] Furthermore, in step S3, after filtering, the filter residue needs to be washed with hot water, and the amount used is 1.5-3 times the weight of the residue.
[0021] The principle of the present invention is as follows: the present invention is aimed at high-calcium clay-type lithium ore, the CaO content is 10%-30%, and CaO mainly exists in the form of calcite, so the chemical dissociation method is first used to remove the CaO (calcite) in the ore, and the lithium chlorite is effectively dissociated and exposed by the reaction of hydrochloric acid or nitric acid with the calcite, which is conducive to the subsequent strong acid leaching of lithium ions in the ore. Then, the wet dissociation slag containing a certain amount of residual acid and the leachate are obtained by direct filtration without washing, and then the wet dissociation slag is subjected to strong acid leaching. The wet dissociation slag plays a role in providing chloride or nitrate in the strong acid leaching process, thereby improving / promoting the effect of the reaction between hydrochloric acid or nitric acid and the mineral lattice, and a high-quality lithium carbonate product can be obtained after subsequent impurity removal.
[0022] The beneficial effects of the present invention are:
[0023] 1) The high-calcium clay-type lithium ore roasting-free leaching process provided by the present invention shortens the production process compared with the conventional roasting-leaching process, solves the problem of high energy consumption of the existing treatment process of high-calcium clay-type lithium ore, enriches the types of available lithium resources, and realizes the effective extraction of lithium from high-calcium clay-type lithium ore. This method also greatly reduces the amount of leached slag, the composition of the leached slag is relatively simple, which is convenient for subsequent comprehensive utilization, and greatly reduces the development and utilization cost of high-calcium clay-type lithium ore.
[0024] 2) The present invention uses hydrochloric acid or nitric acid to chemically dissociate the raw ore, first removing the calcium (calcite) in the ore, destroying the mineral structure of the calcite veins enveloping the lithium chlorite, and at the same time fully exposing lithium chlorite and other lithium-containing minerals, so that the Li in the lithium chlorite + The lattice sites are more easily in contact with the strong acid in the subsequent leaching, thus facilitating the extraction of lithium from the ore into the solution.
[0025] 3) The lithium-rich solid phase product obtained after chemical dissociation and decalcification in the present invention is not dried, but directly added with sulfuric acid for strong acid leaching. High concentration sulfuric acid not only provides a strong acid oxidation environment to destroy the hydrogen bonds between mineral layers, but also + The concentration is greatly increased, increasing the specific surface area between the mineral and the acid interface. + Adsorbed on the lattice surface, catalyzing the reaction between hydrochloric acid or nitric acid and the mineral lattice with Li +Ion exchange is carried out to make the lithium ions in the ore more easily enter the leaching solution.
[0026] 4) Compared with washing filtration, the non-washing filtration of the present invention can greatly retain chloride or nitrate and residual acid in the dissociation slag, so that it is easier to react with the mineral lattice during strong acid leaching, making it easier for lithium ions in the ore to enter the leachate, thereby improving the leaching rate of lithium. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following.
[0029] Example 1
[0030] The main minerals and contents of sedimentary lithium ore in Guizhou are: lithium chlorite (21.10%), quartz (18.48%), calcite (19.10%), pyrite (5.86%), and other minerals, among which the Li2O content is 0.63% and the CaO content is 11.92%. (Hui Bo, Gong Daxing, Chen Wei. Study on the occurrence state of lithium in sedimentary lithium ore in Liuzhi area, Guizhou [J]. Nonferrous Metals (Ore Dressing Part), 2021, 47(11): 1-4)
[0031] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 78%;
[0032] Step 2, chemical dissociation: add 9000 ml of 2 mol / L hydrochloric acid (HCl excess coefficient 4.23) to the sample in step 1, with a liquid-to-solid ratio of 9, and conduct a 5.5 h test at 30°C. By filtering without washing, 1012.25 g of wet dissociation slag is obtained, which contains 4.39% chloride ions and 2.17% residual acid. The calcium impurity is in the leaching solution, and the removal rate reaches 96.73%.
[0033] Step 3, strong acid leaching: the wet dissociation slag with chloride ions and residual acid obtained in step 2 (without drying) is directly put into 3 mol / L sulfuric acid for reaction for 4 hours, the liquid-to-solid ratio is 7 L / kg, the leaching temperature is 120°C, and the lithium-rich leaching solution and aluminum-silicon leaching slag are obtained by filtration, and then 1800 ml of hot water is added to wash the leaching slag, and the obtained washing liquid is reused; the final lithium leaching rate is 92.95%, the Li2O concentration of the leaching solution is as high as 1.05 g / L, and 630.71 g of dry slag is produced, which contains 11.97 g of gypsum, accounting for 1.9%.
[0034] Example 2
[0035] A clay-type lithium ore from Guizhou was used, containing lithium chlorite (18.15%), quartz (26.04%), calcite (18.83%) and other minerals, of which the Li2O content was 0.56% and the CaO content was 23.64%.
[0036] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 60.10%;
[0037] Step 2, chemical dissociation: add 5000 ml of 5 mol / L hydrochloric acid (HCl excess coefficient 2.96) to the sample in step 1, with a liquid-to-solid ratio of 5, and conduct an acid leaching test at 35° C. for 3.5 h. By directly filtering without washing, 848.19 g of wet dissociation slag is obtained, which contains 3.08% chloride ions and 1.83% residual acid. The calcium impurity is in the leaching solution, and the removal rate reaches more than 96.22%;
[0038] Step 3, strong acid leaching: the wet dissociation slag with residual acid obtained in step 2 is not dried, but directly put into 8 mol / L sulfuric acid for reaction for 2 hours, with a liquid-to-solid ratio of 5 L / kg and a leaching temperature of 90°C. The lithium-rich leaching solution and aluminum-silicon leaching slag are filtered out, and 1000 ml of hot water is added to wash the leaching slag, and the washing solution is reused; the final lithium leaching rate is 91.28%, the Li2O concentration of the leaching solution is as high as 1.32 g / L, and 514.42 g of dry slag is produced, of which 27.43 g of gypsum is contained, accounting for 5.33%.
[0039] Example 3
[0040] A clay-type lithium ore from Guizhou was used, containing lithium chlorite (14.83%), quartz (26.84%), calcite (26.72%) and other minerals, of which the Li2O content was 0.58% and the CaO content was 16.74%.
[0041] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 72%;
[0042] Step 2, chemical dissociation: add 6000ml of 3mol / L nitric acid (HNO3 excess coefficient 3.01) to the sample in step 1, with a liquid-to-solid ratio of 6, and perform chemical dissociation at 45°C for 3h. Use a direct filtration method without washing to obtain 947.98g of wet dissociation slag, which contains 2.98% nitrate and 1.43% residual acid. The calcium impurity is in the leaching solution, and the removal rate reaches more than 96.28%;
[0043] Step 3, strong acid leaching: grind the clinker obtained after roasting and cooling in step 2, put it into 3.5 mol / L sulfuric acid for reaction for 4.5 hours, the liquid-to-solid ratio is 3L / kg, the leaching temperature is 100°C, filter to obtain lithium-rich leaching solution and aluminum-silicon leaching residue, add 800 ml of hot water to wash the leaching residue, and reuse the obtained washing solution; the final lithium leaching rate is 91.61%, the Li2O concentration of the leaching solution is as high as 2.23 g / L, and 597.93 g of dry residue is produced, which contains 19.12 g of gypsum, accounting for 3.2%.
[0044] Example 4
[0045] The main minerals and contents of a clay-type lithium mine in the southwest region are: lithium chlorite (16.73%), quartz (21.15%), calcite (39.67%) and other minerals, among which the Li2O content is 0.51% and the CaO content is 29.71%.
[0046] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 90.01%;
[0047] Step 2, chemical dissociation: add 7500ml of 6.5mol / L nitric acid (HNO3 excess coefficient 4.59) to the sample in step 1, with a liquid-to-solid ratio of 7.5, and conduct a 2h 60°C acid leaching test. By directly filtering without washing, 762.66g of wet dissociation slag is obtained, which contains 4.85% nitrate and 2.83% residual acid. The calcium impurity is in the leaching solution, and the removal rate reaches more than 96.98%;
[0048] Step 3, strong acid leaching: the wet dissociation slag with residual acid obtained in step 2 is not dried, but directly put into 2 mol / L sulfuric acid for reaction for 5 hours, the liquid-to-solid ratio is 4 L / kg, the leaching temperature is 80°C, and the lithium-rich leaching solution and aluminum-silicon leaching slag are obtained by filtration, and then 1100 ml of hot water is added to wash the leaching slag, and the obtained washing liquid is reused; the final lithium leaching rate is 92.17%, the Li2O concentration of the leaching solution is as high as 1.68 / L, and 491.03g of dry slag is produced, of which 27.55g of gypsum is contained, accounting for 5.61%.
[0049] Example 5
[0050] A clay-type lithium mine, whose main minerals and contents are: lithium chlorite (14.21%), quartz (22.05%), calcite (42.01%) and other minerals, among which the Li2O content is 0.51% and the CaO content is 28.31%.
[0051] Step 1, grinding: Take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 83%;
[0052] Step 2, chemical dissociation: add 3000ml of 8mol / L hydrochloric acid (HNO3 excess coefficient 2.37) to the sample in step 1, with a liquid-solid ratio of 3, conduct a 6h 50°C acid leaching test, filter without washing, and obtain 778.46g of dissociation slag, which contains 2.78% nitrate and 1.32% residual acid. The calcium impurity is in the leaching solution, and the removal rate reaches more than 96.17%;
[0053] Step 3, strong acid leaching: the wet dissociation slag with residual acid obtained in step 2 is not dried, but directly put into 4 mol / L sulfuric acid for reaction for 6 hours, with a liquid-to-solid ratio of 6L / kg and a leaching temperature of 115°C. The lithium-rich leaching solution and aluminum-silicon leaching slag are filtered to obtain the lithium-rich leaching solution and the aluminum-silicon leaching slag. 1200 ml of hot water is added to wash the leaching slag, and the obtained washing solution is reused. The final lithium leaching rate is 91.03%, the Li2O concentration of the leaching solution is as high as 1.11 g / L, and 505.23 g of dry slag is produced, of which 33.29 g of gypsum is contained, accounting for 6.59%.
[0054] Comparative Example 1 (the main difference from Example 1 is that no chemical dissociation step is performed)
[0055] Using the same clay-type lithium ore from Guizhou as in Example 1, the process steps are as follows:
[0056] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 78%;
[0057] Step 2, strong acid leaching: the ground lithium ore is directly put into 3000 ml of 3 mol / L sulfuric acid to react for 4.5 hours, the leaching temperature is 120°C, and the lithium-rich leaching solution and aluminum-silicon leaching residue are filtered to obtain, and then 1800 ml of hot water is added to wash the leaching residue, and the obtained washing solution is reused; finally, the lithium leaching rate under this condition is 2.14%, and the Li2O concentration of the leaching solution is only 0.04 g / L, and finally 1088.9 g of dry residue is produced, which contains 366.12 g of gypsum, accounting for 33.62%.
[0058] Comparative Example 2 (the main difference from Example 4 is that the chemical dissociation and strong acid leaching steps are combined)
[0059] Using the same clay-type lithium ore from Guizhou as in Example 4, the process steps are as follows:
[0060] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 90.01%;
[0061] Step 2: Prepare a mixed solution of nitric acid and sulfuric acid, which contains 5000 ml of 6.5 mol / L nitric acid and 4000 ml of 2 mol / L sulfuric acid, and put the clay-type lithium ore into the mixed acid solution for reaction for 5 hours, and the leaching temperature is 80° C. Under this condition, the lithium leaching rate is 26.71%, and the Li2O concentration of the leaching solution is only 0.17 g / L, and finally 1300.92 g of dry slag is produced, which contains 669.79 g of gypsum, accounting for 51.46%.
[0062] Comparative Example 3 (the main difference from Example 4 is that the chemical dissociation is replaced by a roasting step)
[0063] Using the same clay-type lithium ore from Guizhou as in Example 4, the process steps are as follows:
[0064] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 90.01%;
[0065] Step 2, roasting: roast the ground ore directly at a temperature of 800°C and a roasting time of 3h;
[0066] Step 3, strong acid leaching: After roasting, the sulfuric acid leaching temperature is 80°C, the leaching time is 6h, the sulfuric acid concentration is 3mol / L, and the leaching liquid-solid ratio is 4 (Note, compared with Example 4, more sulfuric acid is added in this comparative example for sufficient dissociation, because this comparative example does not have a hydrochloric acid dissociation step). The lithium leaching rate under this condition is 93.31%. However, the Li2O concentration of the leachate under this condition is only 1.27g / L, and 1621.3g of slag is finally produced, of which 910.7g of gypsum is contained, accounting for 56.17%.
[0067] Comparative Example 4 (the main difference from Example 2 is that washing and filtration were performed after chemical dissociation)
[0068] Using the same clay-type lithium ore in Guizhou as in Example 2, the process steps are as follows:
[0069] Step 1, grinding: take 1000g of ore and grind it to a particle size of less than 0.074mm, accounting for 60.10%;
[0070] Step 2, chemical dissociation: add 5000 ml of 5 mol / L hydrochloric acid (HCl excess coefficient 2.96) to the sample in step 1, with a liquid-solid ratio of 5, and conduct an acid leaching test at 35° C. for 3.5 hours. The wet dissociation slag obtained by filtering and washing has a chloride content of less than 0.1%;
[0071] Step 3, strong acid leaching: the wet dissociation slag obtained in step 2 is not dried, but directly put into 8 mol / L sulfuric acid for reaction for 2 hours, with a liquid-to-solid ratio of 5 L / kg and a leaching temperature of 90°C. The lithium-rich leaching solution and aluminum-silicon leaching slag are filtered out, and 1000 ml of hot water is added to wash the leached slag, and the obtained washing solution is reused; the lithium leaching rate under this condition is 16.44%, and the Li2O concentration of the leaching solution is only 0.23 g / L, and 519.54 g of slag is finally produced, of which 28.61 g of gypsum is contained, accounting for 5.51%.
[0072] For the convenience of comparison, the applicant organizes the main data involved in the above embodiments and comparative examples into the following table:
[0073] Table 1: Main data parameters of Examples 1-5
[0074]
[0075] It can be seen from the above table that the present invention only adopts a two-leaching process, which not only effectively solves the problem of high energy consumption in the existing clay-type lithium ore processing process, but also realizes the effective extraction of lithium from high-calcium clay-type lithium ore, with a small amount of leached slag and low gypsum content.
[0076] Table 2: Main data parameters of Comparative Examples 1-4, Examples 1, 2, and 4
[0077]
[0078] As can be seen from the above table, the difference between Comparative Example 1 and Example 1 is that the chemical dissociation step is not performed, and Comparative Example 1 cannot achieve effective leaching of lithium. It can be seen that the chemical dissociation step is the key step for the present invention to achieve effective leaching of lithium. The difference between Comparative Examples 2 and 3 and Example 4 is that the chemical dissociation and strong acid leaching steps are combined, and the chemical dissociation is replaced by the roasting step. The experimental results of Comparative Example 2 show that the direct mixed acid leaching has a low lithium leaching rate in high-calcium clay-type lithium ore. Compared with the present invention, there is still a significant gap in the leaching effect, and the amount of leached slag produced by the mixed acid leaching is higher; the experimental results of Comparative Example 3 show that both the chemical dissociation and roasting steps can achieve the effect of dissociation, and the effect of roasting is slightly better, but roasting produces a large amount of dry slag, and also requires a lot of energy consumption. The difference between Comparative Example 4 and Example 2 is that washing is performed, and the chloride ion of the wet dissociation slag is very low. The lithium leaching effect of Comparative Example 4 is greatly reduced, indicating that the non-washing and filtering in the present invention has played an effect of improving lithium leaching.
[0079] Economic Value Analysis
[0080] 1. The process steps of the present invention do not involve a roasting process. According to the research progress of typical lithium-containing mineral roasting and lithium extraction, it is found that according to the theoretical calculation of the roasting system, a roasting rotary kiln is used to process 1 ton of spodumene concentrate, and about 592 kg of standard coal will be consumed. It is worth noting that when semi-industrial experiments are carried out, the consumption of standard coal is at least higher than the theoretical calculation results due to the efficiency of the on-site coal-fired hot air furnace, the insulation effect of the roasting device, and the waste heat recovery capacity. In summary, the roasting process has huge costs and high losses. Especially when conducting industrial experiments, the energy consumption generated by the roasting process is very huge, and this is the result of not considering the purchase of roasting equipment and equipment loss.
[0081] 2. This patent follows the concept of energy conservation and emission reduction, reduces the roasting process, greatly reduces energy consumption and the emission of waste gases such as carbon dioxide, especially if the ore contains S elements, SO2 will be produced, which will greatly pollute the environment.
[0082] 3. The present invention greatly reduces the generation of gypsum by adding a chemical dissociation process. It can be seen from the comparative examples of this patent that a large amount of gypsum will be produced if the high-calcium clay-type lithium ore adopts the previous process. Gypsum not only makes the leached slag difficult to handle, greatly reducing the availability of the slag, but also occupies land and wastes resources. The acidity and other harmful substances contained in it are easy to pollute the surrounding environment. In the existing actual industrial production, phosphogypsum has become an important factor restricting the sustainable development of my country's phosphorus chemical enterprises.
[0083] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.
Claims
1. A low-cost lithium extraction process without roasting of high-calcium clay-type lithium ore, characterized in that: It consists of the following steps: S1. Grinding: Grind the high calcium clay-type lithium ore to -0.074mm, accounting for 60%-90%; Wherein, the Li2O content in the high calcium clay-type lithium ore is less than 1%, and the CaO content is 10%-30%; S2, chemical dissociation: adding the ground high-calcium clay-type lithium ore to hydrochloric acid or nitric acid for chemical dissociation, and filtering directly without washing after the chemical dissociation to obtain wet dissociation slag and dissociation liquid; The concentration of the hydrochloric acid or nitric acid is 2-8 mol / L, the liquid-solid ratio of chemical dissociation is 3-9 L / kg, the temperature is 30°C-90°C, and the time is 2-6 hours; the chloride or nitrate content in the wet dissociation slag is 2.5-5%, and the residual acid content is 1-3%; S3, strong acid leaching: the wet dissociation residue is subjected to strong acid leaching with sulfuric acid, and filtered to obtain lithium-rich leaching solution and aluminum-silicon leaching residue; The concentration of sulfuric acid is 2-6 mol / L, the liquid-to-solid ratio of strong acid leaching is 3-7 L / kg, the temperature is 80° C.-120° C., and the time is 1.5-6 h.
2. A high calcium clay type lithium ore free roasting and low cost lithium extraction process according to claim 1, characterized in that: In step S2, the dissociation liquid is used as a high-calcium clay-type lithium ore after mixed grinding with hydrochloric acid or nitric acid for preliminary dissociation. After preliminary dissociation and filtration, preliminary dissociation slag and preliminary dissociation liquid are obtained. The preliminary dissociation liquid slag can be used as a raw material for chemical dissociation.
3. The process for extracting lithium from high-calcium clay-type lithium ore without roasting and at low cost according to claim 1, characterized in that: In step S2, the concentration of the hydrochloric acid or nitric acid is 3-6 mol / L, and the liquid-solid ratio of chemical dissociation is 4-6 L / kg.
4. The process for extracting lithium from high-calcium clay-type lithium ore without roasting and at low cost according to claim 1, characterized in that: In step S2, the temperature of the chemical dissociation is 50°C-80°C, and the time is 3-5h.
5. The process for extracting lithium from high-calcium clay-type lithium ore without roasting and at low cost according to claim 1, characterized in that: In step S2, the chloride or nitrate content in the wet dissociation residue without washing and filtering is 3-4.5%, and the residual acid content is 1.5-2.5%.
6. The process for extracting lithium from high-calcium clay-type lithium ore without roasting and at low cost according to claim 1, characterized in that: In step S3, the temperature of the strong acid leaching is 90°C-105°C, and the time is 3-5h.
7. The process for extracting lithium from high-calcium clay-type lithium ore without roasting and at low cost according to claim 1, characterized in that: In step S3, the concentration of the sulfuric acid solution is 3-5 mol / L, and the liquid-to-solid ratio of strong acid leaching is 4-6 L / kg.
8. The process for extracting lithium from high-calcium clay-type lithium ore without roasting and at low cost according to claim 1, characterized in that: In step S3, after filtering, the filter residue needs to be washed with hot water, and the amount used is 1.5-3 times the weight of the residue.
Citation Information
Patent Citations
Method for directly preparing lithium sulfate from hard rock type lithium ore
CN114368764A
Method for extracting lithium ions from clay-type lithium ore with extremely low lithium grade by ion substitution
CN115976337A
Method for leaching lithium in clay type lithium ore by using recyclable solid acid
CN116065037A
Method for separating and extracting lithium in carbonate clay type lithium ore
CN116179874A
Method for selectively leaching lithium from clay type lithium ore
CN116240399A