Automobile wheel hub coating and preparation method and application thereof
By using a combined coating structure of epoxy polyester powder coating, water-based polyester resin and water-based modified inorganic nanocoating on the surface of automotive aluminum alloy wheel hubs, the problems of poor corrosion resistance and insufficient wear resistance of existing coatings are solved, and the problem of insufficient corrosion resistance of existing coatings is achieved. Coating effect with high hardness, weather resistance and self-healing functions.
Patent Information
- Application Number
- CN202311427899.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-10-31
AI Technical Summary
The existing automotive aluminum alloy wheel hub coatings have problems such as poor corrosion resistance, insufficient wear resistance and easy cracking. Especially due to the high roughness of the aluminum alloy surface and the presence of iron-silicon elements, the adhesion of ceramic coatings is reduced, and it is unable to effectively cover up unevenness. surface.
The powder coating layer, primer layer and topcoat layer structure are arranged in sequence, and the powder coating layer is epoxy polyester powder coating, the primer layer contains aqueous polyester resin, aqueous acrylic resin and water-based closed isocyanate, and the topcoat is The layer of aqueous modified inorganic nanocoating and aqueous organosilane dispersion is enhanced by combining and crosslinking these components.
It achieves effective covering and corrosion protection on the surface of aluminum alloy wheel hubs, improves the anti-aging, hardness, wear resistance, scratch resistance and acid and alkali resistance of the coating, extends the service life, and has self-healing function.
Smart Images

Figure BDA0004522774490000161 
Figure BDA0004522774490000162 
Figure BDA0004522774490000163
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of automobile wheel hub coatings, in particular to an automobile wheel hub coating and a preparation method and application thereof. Background Art
[0002] At present, the surface coating of automobile wheels is basically an organic coating, usually a three-layer coating of primer-color paint-clear varnish or primer-color paint-transparent powder; among which, the clear varnish is mainly acrylic amino paint, and the transparent powder is mainly glycidyl methacrylate acrylic powder. Automobile wheels are exposed to the outdoor environment for a long time. With the impact of various media such as dust, sand, rain, and light exposure in the outdoor environment on the surface coating of the wheel hub, the coating structure of the existing automobile wheel hub is prone to reduced color retention, easy to be stained with dust, obvious stone impact marks, and reduced wear resistance, which affects the service life and aesthetics of the wheel hub.
[0003] Nano water-based ceramic coatings prepared by the sol-gel method have the advantages of anti-aging, high hardness, wear resistance, scratch resistance, acid and alkali resistance, etc., and have been relatively mature in use on the surface of aluminum veneers. This feature is also the function required by existing automotive aluminum alloy wheel hub coatings. If nano water-based ceramic coatings can be applied to the surface of aluminum alloy wheels, the shortcomings of existing technologies will be solved.
[0004] However, the existing automotive aluminum alloy wheels are mainly A356 series cast aluminum alloys. The surface roughness of the cast aluminum alloy wheels is relatively high, and there are many pinholes on the surface. In addition, this series of aluminum alloys is more prone to filiform corrosion than aluminum veneers for construction. If water-based ceramic coatings are directly applied to the surface of automotive aluminum alloy wheels, although the shortcomings of the organic coatings of existing automotive aluminum alloy wheels can be improved, the water-based ceramic coatings cannot be sprayed too thick. If they are too thick, the water-based ceramic coatings themselves are prone to cracking, and there is a risk of decreased adhesion. The casting surface roughness of A356 cast aluminum alloy is high, and it is impossible to spray too thick ceramic coatings, resulting in uneven coatings formed on the surface of the automotive wheel. At the same time, A356 cast aluminum alloys are prone to corrosion due to the presence of elements such as iron and silicon. The thickness of the ceramic coating is not enough to cover the uneven surface of the aluminum alloy, and it is easy to have problems such as unsatisfactory coating appearance, decreased adhesion, long-term corrosion resistance, and insufficient wear resistance. Therefore, there are many disadvantages in simply applying water-based ceramic coatings directly to the surface of automotive aluminum alloy wheels. Summary of the invention
[0005] Based on this, the purpose of the present invention is to provide a coating for automobile wheel hub and its preparation method and application. The automobile wheel hub coating of the present invention can not only cover the rough surface of the automobile aluminum alloy wheel hub and provide anti-corrosion performance, but also achieve many advantages of existing ceramic coatings.
[0006] The present invention adopts the following technical solutions:
[0007] An automobile wheel hub coating comprises a powder coating layer, a primer layer, and a topcoat layer which are sequentially arranged on the surface of the automobile wheel hub;
[0008] The powder coating layer is formed by coating the powder coating on the surface of the automobile wheel hub; the powder coating is epoxy polyester powder coating;
[0009] The primer layer is formed by a primer; the primer comprises the following components in mass percentage: 20-30% water-based polyester resin; 5-10% water-based acrylic resin; 5-15% water-based blocked isocyanate; 0.1-2.5% neutralizer; 0.1-0.5% substrate wetting agent; 0.1-0.5% leveling agent; 0.2-0.8% defoamer; 0.1-1.0% thickener; 2-6% cosolvent; the balance is deionized water;
[0010] The topcoat layer is formed by a topcoat; the topcoat comprises the following components in percentage by mass: 85-95% of a water-based modified inorganic nano coating, 5-8% of a water-based organic silane dispersion, and the balance of deionized water;
[0011] in:
[0012] The water-based modified inorganic nano coating comprises the following components in percentage by mass: 55-75% of water-based modified nano dispersion, 5-25% of pigment, 0.2-3% of wetting dispersant, 0.5-2% of leveling agent, 0.1-0.8% of defoamer, 0.1-0.9% of thickener, and the balance of deionized water;
[0013] The aqueous nano-modified dispersion comprises the following components in percentage by mass: 40-50% aqueous nano-silicon dioxide dispersion, 25-35% alkoxysilane, 10-30% aqueous polyester dispersion, 0.5-5% anionic surfactant, and the balance deionized water;
[0014] The aqueous organic silane dispersion comprises the following components in percentage by mass: 45-65% aminosilane, 0.5-5% anionic surfactant, and the balance deionized water.
[0015] The automobile wheel hub coating of the present invention meets the requirements of corrosion resistance and covering fur defects of automobile aluminum alloy wheels by arranging a powder coating layer, a primer layer, and a topcoat layer on the surface of the automobile wheel hub, which can not only improve the covering and corrosion resistance, but also achieve many advantages of ceramic coatings. In the automobile wheel hub coating of the present invention, the powder coating layer is formed by coating the surface of the automobile wheel hub with epoxy polyester powder coating, which can cover the rough surface of the automobile aluminum alloy wheel hub and provide corrosion resistance, meet the requirements of corrosion resistance and covering fur defects of the automobile aluminum alloy wheel hub; then the primer layer and the topcoat layer formed by coating the primer and the topcoat respectively on the surface of the powder coating layer, through the primer layer and the topcoat layer, the covering and corrosion resistance can be improved, and many advantages of existing ceramic coatings can be achieved, with excellent anti-aging, high hardness, wear resistance, scratch resistance, acid and alkali resistance and other advantages. The primer layer plays a role of "bridging the gap" and plays a key role in the bonding strength between the topcoat layer and the powder coating layer, so that the bonding strength between the powder coating layer, the primer layer and the topcoat layer is guaranteed, and the topcoat layer can have high wear resistance, high hardness and weather resistance.
[0016] The primer layer of the present invention is mainly composed of water-based polyester resin, water-based acrylic resin and water-based blocked isocyanate; the water-based polyurethane resin has excellent bonding strength with the epoxy polyester powder coating in the powder coating layer, so that the bonding strength between the primer layer and the powder coating layer is improved; the water-based blocked isocyanate is selected for cross-linking, so that the elasticity of the primer layer is moderate; within the curing range of the primer layer of the present invention, the water-based acrylic resin is more suitable than the amino type resin, and the water-based acrylic resin plays a role in improving the bonding strength with the powder coating layer and the topcoat layer, and strengthens the bonding between the water-based polyester resin in the primer layer and the epoxy resin in the powder coating layer The water-based acrylic resin can enhance the reaction activity in the primer component, enhance the reaction activity between the water-based polyester resin and the water-based blocked isocyanate, and make the elasticity of the primer layer more moderate; in addition, the water-based blocked isocyanate in the primer layer can react with the hydroxyl group in the topcoat, and the water-based polyester resin in the primer layer and the hydroxyl group in the water-based acrylic dispersion can also participate in the reaction in the topcoat, so that the bonding force between the primer layer and the topcoat layer is guaranteed, and the existing topcoat mainly made of inorganic materials and containing a large amount of inorganic pigments and fillers is difficult to ensure the low bonding force and poor long-term effect with the powder coating layer in the absence of the organic coating primer layer. The water-based acrylic resin in the primer and the water-based polyester resin contain a large amount of active hydroxyl groups, which can react with the water-based blocked isocyanate in the primer, and can also react with the alkoxysilane and aminosilane in the topcoat, while achieving cross-linking within the layer, it can also promote cross-linking between layers, further enhancing the bonding force of the components within the primer layer and the bonding force between the topcoat and the primer layer.
[0017] In the topcoat layer of the present invention, alkoxysilane is used as a precursor for the reaction, nano-silicon dioxide is used as a reinforcing phase, and alkoxysilane monomers and nano-silicon dioxide are mixed in a liquid phase to form a stable and uniform transparent system. During the aging process of the mixed system, the alkoxysilane monomer undergoes hydrolysis and self-condensation reaction in the water phase, and the condensation product and nano-silicon dioxide particles undergo condensation reaction again. The components in the system undergo slow polymerization to generate a large number of spatial network structures, and then the solvent water in the network structure is volatilized through heat treatment to finally form a coating containing nano-silicon dioxide particles. Compared with the organic coating on the surface of the existing automobile aluminum alloy wheel hub, the automobile wheel hub coating of the present invention introduces inorganic nanomaterials into the topcoat, so that the wear resistance, weather resistance, hardness, etc. of the coating are significantly improved, the low surface energy of the coating and the ability of the inorganic material to eliminate static electricity are improved, so that the coating will not absorb pollutants in the atmosphere and always maintain a clean appearance, solving the shortcomings of the existing organic coatings such as poor wear resistance, poor weather resistance such as light retention and color retention. The water-based polyester dispersion in the topcoat contains a large amount of active hydroxyl groups, which can react with the alkoxysilane and aminosilane in the topcoat, and can also react with the water-based blocked isocyanate in the primer. While promoting the intralayer crosslinking of the topcoat layer, it can also promote the crosslinking with the primer layer, further improving the bonding strength. The addition of the water-based polyester dispersion reduces the shrinkage stress of the inorganic coating, greatly reduces the risk of cracking of the coating after baking and the risk of cracking of the coating over time. The hardness, wear resistance and other properties of the resulting coating are greatly improved compared to pure organic coatings.
[0018] The present invention forms the automobile wheel hub coating on the surface of the automobile wheel hub, that is, sequentially forms a powder coating layer, a primer layer, and a topcoat layer on the surface of the automobile wheel hub, thereby improving the problems existing in the prior art in which water-based ceramic coatings are directly applied to the surface of the automobile wheel hub, and can meet the requirements of the corrosion resistance of the automobile wheel hub and covering fur defects, and can improve the covering and corrosion resistance, and has the advantages of excellent anti-aging, high hardness, wear resistance, scratch resistance, acid and alkali resistance, etc.
[0019] As an improvement of the above scheme, the aqueous nano-modified dispersion also includes the following components in mass percentage: 5-8% aqueous acrylic resin microcapsules, 5-8% isocyanate microcapsules; the aqueous acrylic resin microcapsules include a first wall material and a first core material, the first wall material includes urea-formaldehyde resin, and the first core material includes aqueous acrylic resin; the isocyanate microcapsules include a second wall material and a second core material, the second wall material includes nano-silicon dioxide, the second core material includes isocyanate, and the isocyanate is aqueous isocyanate. The present invention takes into account the risk of cracking of the automotive wheel hub coating after baking and the risk of cracking of the coating over time, as well as the bonding strength and long-term effectiveness between the topcoat layer and the primer layer, and adds aqueous acrylic resin microcapsules and isocyanate microcapsules to the topcoat layer to ensure the bonding strength and long-term stability between the powder coating layer, the primer layer, and the topcoat layer. Among them, according to the above content, it can be known that the water-based acrylic resin in the primer layer can play a role in improving the bonding force between the powder coating layer and the primer layer. The water-based acrylic resin in the primer layer can also react with the water-based blocked isocyanate in the primer layer. At the same time, the water-based acrylic resin in the primer layer can also react with the alkoxysilane and aminosilane in the topcoat. Therefore, the water-based acrylic resin in the primer layer can promote cross-linking within the primer layer while promoting cross-linking between layers, thereby improving the bonding force between layers. In order to reduce the risk of cracking of the coating after baking and the risk of cracking of the coating over time in the later period, and to ensure the bonding force and long-term effectiveness between the topcoat layer and the primer layer, the isocyanate microcapsules are added to the topcoat. The nano-silicon dioxide on the second wall material of the isocyanate microcapsules can participate in the reaction of the hydrolysis and polycondensation products of the alkylsiloxane, further polymerizing and generating a large number of spatial network structures in the topcoat layer, further enhancing the stability of the coating of the nano-silicon dioxide particles; in addition, the present invention also adds the water-based acrylic resin microcapsules to the topcoat. When the automobile wheel hub coating is stressed and cracked, the water-based acrylic resin microcapsules The first wall material and the second wall material of the isocyanate microcapsule are subjected to stress and cracks appear, the water-based acrylic resin microcapsules release the water-based acrylic resin, the isocyanate microcapsules can release the isocyanate through the pore structure of nano-silicon dioxide or the rupture of the microcapsules themselves, the isocyanate in the isocyanate microcapsules reacts with the water-based acrylic resin released from the water-based acrylic resin microcapsules to cause the cracks to re-bond, thereby achieving self-repair of the automobile wheel hub coating, greatly extending the service life of the automobile wheel hub coating, and ensuring the bonding strength and long-term stability between the powder coating layer, the primer layer, and the topcoat layer.In addition, when each is broken, the aqueous acrylic resin released from the aqueous acrylic resin microcapsules may also react with the alkoxysilane and aminosilane in the topcoat, and may also react with the aqueous blocked isocyanate in the primer, further bonding the cracks and further strengthening the bonding force with the primer layer, reducing the risk of cracking of the coating, and greatly improving the hardness and wear resistance of the resulting topcoat layer. The isocyanate released from the isocyanate microcapsules may also react with the aqueous polyester dispersion in the topcoat, further bonding the cracks and strengthening the bonding strength in the topcoat layer. In some preferred embodiments, the first core material of the aqueous acrylic resin microcapsules also includes a crosslinking promoter, such as a photoinitiator or other crosslinking promoter, which accelerates the reaction of the aqueous acrylic resin released from the rupture of the aqueous acrylic resin microcapsules with other components to increase the bonding speed and further reduce the risk of cracking of the coating.
[0020] For the convenience of describing the waterborne acrylic resin microcapsules and isocyanate microcapsules of the present invention, the waterborne acrylic resin microcapsules and isocyanate microcapsules of the present invention can be prepared by existing microcapsule preparation methods, such as template method, interfacial polycondensation method, in-situ polymerization method, etc. The following is only used to introduce the preferred preparation method, and those skilled in the art can prepare the corresponding method according to the existing common knowledge, which will not be repeated here.
[0021] As a preferred preparation method of the water-based acrylic resin microcapsules, the method comprises the following steps: mixing and stirring a first core material (including a water-based acrylic resin) and an emulsifier to obtain a first core material emulsion; preparing a urea-formaldehyde resin solution, adding the urea-formaldehyde resin solution dropwise into the first core material emulsion, adjusting the pH to 2.5-3 and heating to 65-75°C for reaction, standing, washing, and drying to obtain water-based acrylic resin microcapsules.
[0022] A preferred preparation method of the isocyanate microcapsules comprises the following steps: using an aqueous dispersion of nano-silicon dioxide as an aqueous phase; using an organic mixed liquid containing a second core material (including aqueous isocyanate) as an oil phase; mixing the oil phase with the aqueous phase and emulsifying the mixture to prepare an oil-in-water emulsion; adding a cross-linking agent to the prepared emulsion for reaction, standing, filtering, washing and drying to obtain isocyanate microcapsules.
[0023] As a preferred solution, in the primer, the water-based polyester resin is a water-soluble polyester resin, with a solid content of 60-80%, a hydroxyl content of 90-150 mgKOH / g, and the hydroxyl content is the hydroxyl content when converted to 100% resin solids; in the topcoat, the solid content of the water-based polyester dispersion is 30-50%, and the hydroxyl content is 60-120 mgKOH / g, and the hydroxyl content is the hydroxyl content when converted to 100% resin solids, and the pH value is 7.0-9.0. In common knowledge, water-based polyester resins mainly include water-soluble polyester resins, water-based polyester dispersions, and water-based polyester emulsions. The present invention uses a water-soluble polyester resin in the primer, and the resin contains a certain amount of cosolvent, which is relatively easy to infiltrate the surface of the powder coating layer. At the same time, there is no need to add an overly strong wetting and leveling agent in the primer, which is conducive to the subsequent topcoat coating on the sprayed primer; and the present invention uses a water-based polyester dispersion in the topcoat, and this type of resin has relatively good miscibility with the subject component in the topcoat. The present invention takes into account the binding force between the waterborne polyester resin in the primer and the epoxy polyester powder coating, the reactivity with the waterborne blocked isocyanate in the primer, and the reaction with the components in the topcoat, and designs the hydroxyl content of the waterborne polyester resin in the primer to be 90-150 mgKOH / g, which not only ensures the binding force with the powder coating layer, but also ensures the crosslinking density in the primer layer, and can enhance the binding force between the primer layer and the topcoat layer. In the topcoat, the hydroxyl content of the waterborne polyester dispersion is 60-120 mgKOH / g. This aspect takes into account the crosslinking density of the waterborne polyester dispersion in the topcoat and the reaction with the waterborne blocked isocyanate in the primer, and designs the hydroxyl content of the waterborne polyester dispersion in the topcoat to be 60-120 mgKOH / g, which reduces the risk of cracking of the topcoat layer after baking and the cracking of the coating layer over time, greatly improves the hardness and wear resistance of the coating, and improves the binding force with the primer layer. Preferably, the water-soluble polyester resin is Tongde 1PB83Y; and the water-based polyester dispersion is Tongde 3PB811W.
[0024] As a preferred solution, the nano-silicon dioxide aqueous dispersion has a solid content of 25-35%, an average particle size of 10-110 nm, and a pH value of 7-10. In order to facilitate the polycondensation reaction between the polycondensation product of the alkoxysilane in the topcoat and the nano-silicon dioxide particles, a nano-silicon dioxide aqueous dispersion with a solid content of 25-35%, an average particle size of 10-110 nm, and a pH value of 7-10 is selected, so that the spatial network structure generated by the system polymerization and the topcoat layer containing the nano-silicon dioxide particles have excellent anti-aging, high hardness, wear resistance, scratch resistance, acid and alkali resistance and other properties.
[0025] As a preferred solution, the alkoxysilane is: methyltrimethoxysilane, methyltriethoxysilane or a mixture of the two. The above-mentioned alkoxysilane is used to facilitate hydrolysis and polycondensation after hydrolysis, so that the polycondensation product can repolymerize the nano-silica particles.
[0026] Furthermore, the anionic surfactant is at least one of a carboxylate type, a sulfonate type, a sulfate (ester) type and a phosphate (ester) type.
[0027] Furthermore, the pigment is at least one of titanium dioxide, copper chrome black, cobalt blue, manganese iron black, and metallic pigments.
[0028] Furthermore, the leveling agent is a polyacrylate solution (for example, BYK-346 can be used); the defoamer is at least one of a silicone defoamer or a mixture of hydrophobic particles and a foam-breaking polymer (for example, BYK-028 can be used); and the thickener is at least one of a pseudoplastic polyurethane thickener or a Newtonian polyurethane thickener (for example, BorchiGel0620 or Borchi Gel 0434 can be used).
[0029] Furthermore, the aminosilane is at least one of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.
[0030] Furthermore, the water-based acrylic resin is a water-soluble acrylic resin, with a solid content of 55-75% and a hydroxyl content of 60-90 mgKOH / g, wherein the hydroxyl content is the hydroxyl content when converted to 100% resin solids. The present invention takes into account the reactivity and crosslinking density in the components of the primer, as well as the bonding between the water-based polyester resin in the primer layer and the epoxy resin powder coating of the powder coating layer, and designs the water-based acrylic resin to be a water-soluble acrylic resin, with a solid content of 55-75% and a hydroxyl content of 60-90 mgKOH / g, so as to improve the bonding between the primer layer and the powder coating layer, increase the crosslinking density in the primer layer, and increase the bonding between the primer layer and the topcoat layer. Preferably, the water-soluble acrylic resin is Tongde 1AB911Y.
[0031] Furthermore, the water-based blocked isocyanate is of HDI type, with a solid content of 65%-85%, an NCO content of 8-11%, and a deblocking temperature of 100-120°C. The use of the above-defined water-based blocked isocyanate can facilitate the cross-linking of the internal components of the primer layer and the cross-linking with the components of the topcoat layer to form a layer structure with strong adhesion. Preferably, the water-based blocked isocyanate is selected from Huiyu HY112.
[0032] Furthermore, the neutralizer is N,N-dimethylethanolamine, the leveling agent is a polyacrylate solution, the substrate wetting agent is a polyether-modified siloxane solution, the defoamer is at least one of an organic silicon defoamer or a mixture of hydrophobic particles and a foam-breaking polymer, and the thickener is at least one of a pseudoplastic polyurethane thickener or a Newtonian polyurethane thickener.
[0033] Furthermore, the co-solvent is a mixture of an alcohol ether solvent and an alcohol solvent, wherein the alcohol ether solvent is at least one of ethylene glycol butyl ether, diethylene glycol butyl ether or propylene glycol methyl ether, and the alcohol solvent is at least one of ethanol, isopropanol and n-butanol.
[0034] The present invention also provides a method for preparing any of the above-mentioned automobile wheel hub coatings, comprising the following steps:
[0035] S1: spraying the powder coating on the surface of the automobile wheel hub and curing it at 160-200°C to form a powder coating layer with a thickness of 50-90 μm;
[0036] S2: spraying primer and topcoat respectively on the surface of the powder coating layer obtained in S1, and curing at 120-130° C. to form a primer layer and a topcoat layer respectively, wherein the thickness of the primer layer is 3-8 μm, and the thickness of the topcoat layer is 15-30 μm; thereby obtaining the automobile wheel hub coating.
[0037] In the preparation method of the automobile hub coating of the present invention, powder coating is sprayed on the surface of the automobile hub and cured at 160-200°C according to the curing requirements of the powder coating. The thickness of the powder coating layer is controlled at 50-90μm. If the thickness is too low, the defects of the blank and the anti-corrosion requirements cannot be covered. If the thickness is too high, the overall coating will easily crack due to the difference in shrinkage rate over time. Then, the surface of the powder coating layer obtained in S1 is coated with primer and topcoat by spraying, and cured at 120-130°C. The primer and topcoat are cured at one time to obtain a primer layer and a topcoat layer, respectively, so as to obtain the automobile hub coating. The thickness of the primer layer is 3-8μm. If the thickness of the primer layer is too high, the hardness and physical and chemical properties of the overall coating are easily reduced. If the thickness of the primer layer is too low, it does not play a role in improving adhesion. The thickness of the topcoat layer is 15-30μm. If the thickness of the topcoat layer is too high, the shrinkage stress of the paint film is too large, and the coating is easy to crack. If the thickness of the topcoat layer is too low, the properties such as wear resistance do not reach the ideal state.
[0038] Further, S1, before spraying the powder coating, the automobile wheel hub (automobile aluminum alloy wheel hub) is subjected to chromium-free pretreatment after casting and processing.
[0039] As a preferred preparation method of the primer, the method comprises the following steps:
[0040] (1) Pre-adding water-based polyester resin, water-based acrylic resin, cosolvent, and part of deionized water into a container, slowly dropping a neutralizer in a dispersed state and dispersing it uniformly;
[0041] (2) Add the substrate wetting agent, leveling agent, defoamer, and thickener in a dispersed state and disperse them evenly;
[0042] (3) adding water-based blocked isocyanate and the balance of deionized water and dispersing them evenly;
[0043] (4) The pH value is adjusted to 8.0-9.5 with a neutralizer, and the primer is obtained after mixing evenly.
[0044] As a preferred preparation method of the topcoat, the method comprises the following steps:
[0045] (I) After one or more alkoxysilanes are mixed evenly, an anionic surfactant is added and stirred until it is evenly dispersed in the alkoxysilane to form a translucent mixed liquid a; an aqueous polyester resin dispersion and deionized water are added to the nano-silicon dioxide aqueous dispersion and stirred evenly to obtain a mixed liquid b; the mixed liquid a is slowly added dropwise to the mixed liquid b for 15-25 minutes, then the temperature is raised to 40-65°C, the reaction is carried out at a constant temperature for 1-5 hours, and the heating is stopped and the temperature is lowered to room temperature to obtain an aqueous nano-modified dispersion c;
[0046] (II) mixing the aqueous nano-modified dispersion c prepared in (I) with a pigment, a wetting dispersant, a defoaming agent, a leveling agent and part of deionized water, dispersing the mixture with a high-speed disperser for 10-30 min, and then grinding the mixture with a sand mill, controlling the temperature of the grinding base material to be below 63° C., adding a thickener and the remaining amount of deionized water after the fineness requirement is reached, and dispersing the mixture uniformly to obtain an aqueous modified inorganic nano-coating;
[0047] (III) Mix one or more anionic surfactants with water, mix them evenly, then slowly drop the aminosilane into the aqueous solution of the anionic surfactant for 15-25 minutes. After the dropwise addition is completed, continue to disperse for 1-2 hours, cool to room temperature, and obtain an aqueous silicone dispersion;
[0048] (IV) Mixing the water-based modified inorganic nano-coating obtained in (II) with the water-based organosilicon dispersion obtained in (III), and dispersing at a low speed for 20-30 minutes after mixing to obtain the topcoat.
[0049] Furthermore, when the water-based acrylic resin microcapsules and the isocyanate microcapsules are also used in the topcoat: in step (I), the water-based polyester resin dispersion, the water-based polyester resin microcapsules, the isocyanate microcapsules and deionized water are added to the nano-silicon dioxide aqueous dispersion and stirred evenly to obtain the mixed liquid b.
[0050] The invention also provides an application of an automobile wheel hub coating on the surface of an automobile aluminum alloy wheel hub.
[0051] Furthermore, the automobile aluminum alloy wheel hub is an automobile aluminum alloy wheel hub cast in A356 series.
[0052] Due to the high roughness of the casting surface of A356 cast aluminum alloy, it is impossible to spray too thick ceramic coating on the surface, which will appear uneven. At the same time, A356 cast aluminum alloy is prone to corrosion due to the presence of elements such as iron and silicon. The thickness of the ceramic coating is not enough to cover the uneven surface of the aluminum alloy, so it is easy to have problems such as poor corrosion resistance. The automobile wheel hub coating of the present invention is used for the cast automobile aluminum alloy wheel hub of the A356 series to cover the rough surface and provide anti-corrosion performance, and achieve many advantages of ceramic coatings, such as anti-aging, high hardness, wear resistance, scratch resistance, acid and alkali resistance, etc. DETAILED DESCRIPTION
[0053] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details of this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0054] The present invention is further described below in conjunction with the examples, which are only used to illustrate the present invention and are not used to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually carried out according to conventional conditions in the art or according to the conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets. Any non-substantial changes and replacements made by those skilled in the art on the basis of the present invention belong to the scope of protection claimed by the present invention. In Examples 4-6, the water-based acrylic microcapsules and isocyanate microcapsules are both existing products, and the water-based acrylic microcapsules used are microcapsules with reference to CN107715811B; the isocyanate microcapsules used are microcapsules of CN109535315B. Those skilled in the art can select other types of water-based acrylic resin microcapsules containing urea-formaldehyde resin in the wall material and water-based acrylic resin in the core material, as well as isocyanate microcapsules containing nano-silica in the wall material and isocyanate in the core material as needed.
[0055] For the convenience of expression, 5 tables are used below to express the proportions and product performances of 6 implementation methods, which are respectively the raw material components and mass percentages of the primer and topcoat in the automobile wheel hub coating of Examples 1-6; please understand the present invention in conjunction with Tables 1-5 and the contents of specific Examples 1-6.
[0056] Example 1
[0057] This embodiment provides a car wheel hub coating, comprising a powder coating layer, a primer layer, and a topcoat layer sequentially arranged on the surface of the car wheel hub.
[0058] The powder coating layer is formed by coating the powder coating on the surface of the automobile wheel hub; the powder coating is epoxy polyester powder coating.
[0059] The primer layer is formed by a primer; the primer comprises the following components in percentage by mass:
[0060] Water-based polyester resin (water-soluble polyester resin, Tongde 1PB83Y) 30%;
[0061] Water-based acrylic resin (water-soluble acrylic resin, Tongde 1AB911Y) 8%;
[0062] Water-based blocked isocyanate (Hui Yu HY112) 10%;
[0063] Neutralizer (N,N-dimethylethanolamine) 1%;
[0064] Substrate wetting agent (polyether modified siloxane solution) 0.3%;
[0065] Leveling agent (BYK-346) 0.3%
[0066] Defoamer (BYK-011) 0.5%;
[0067] Thickener (Borchi Gel 0620) 0.8%;
[0068] Cosolvent (mixture of 50wt% ethylene glycol butyl ether and 50wt% ethanol) 5%;
[0069] Deionized water balance.
[0070] The topcoat layer is formed by a topcoat, and the topcoat includes the following components in percentage by mass:
[0071] Water-based modified inorganic nano coating 90%;
[0072] Aqueous organosilane dispersion 7%;
[0073] Deionized water balance.
[0074] in:
[0075] The aqueous organosilane dispersion comprises the following components in percentage by mass:
[0076] Aminosilane (3-aminopropyltrimethoxysilane) 65%;
[0077] Anionic surfactant (carboxylate type anionic surfactant) 5%,
[0078] Deionized water balance.
[0079] The water-based modified inorganic nano coating comprises the following components in percentage by mass:
[0080] Aqueous nano-modified dispersion 65%;
[0081] Pigment (titanium dioxide) 15%;
[0082] Wetting and dispersing agent 2%;
[0083] Leveling agent (BYK-346) 1%;
[0084] Defoamer (BYK-028) 0.5%;
[0085] Thickener (Borchi Gel 0620) 0.5%;
[0086] Deionized water balance.
[0087] Wherein: the aqueous nano-modified dispersion comprises the following components in percentage by mass:
[0088] Nano-silicon dioxide aqueous dispersion (solid content 30%, average particle size 80nm, pH value 8) 50%;
[0089] Alkoxysilane (methyltrimethoxysilane) 30%,
[0090] Water-based polyester dispersion (Tongde 3PB811W) 10%,
[0091] Anionic surfactant (carboxylate type anionic surfactant) 3%,
[0092] Deionized water balance.
[0093] This embodiment also provides a method for preparing a coating on a vehicle hub, comprising the following steps:
[0094] The present invention also provides a method for preparing any of the above-mentioned automobile wheel hub coatings, comprising the following steps:
[0095] S1: spraying the powder coating on the surface of the automobile wheel hub and curing it at 160-200°C to form a powder coating layer with a thickness of 80 μm;
[0096] S2: spraying primer and topcoat respectively on the surface of the powder coating layer obtained in S1, and curing at 120-130° C. to form a primer layer and a topcoat layer respectively, wherein the thickness of the primer layer is 8 μm, and the thickness of the topcoat layer is 25 μm; thereby obtaining the automobile wheel hub coating.
[0097] Wherein: the preparation method of the primer comprises the following steps:
[0098] (1) Add water-based polyester resin, water-based acrylic resin, cosolvent, and part of deionized water into a container in advance according to the proportion, and slowly dropwise add the neutralizer in a dispersed state and disperse it evenly;
[0099] (2) Add the substrate wetting agent, leveling agent, defoamer, and thickener in a dispersed state and disperse them evenly;
[0100] (3) adding water-based blocked isocyanate and the balance of deionized water and dispersing them evenly;
[0101] (4) The pH value is adjusted to 8.0-9.5 with a neutralizer, and the primer is obtained after mixing evenly.
[0102] The preparation method of the topcoat comprises the following steps:
[0103] (I) adding alkoxysilane to anionic surfactant according to the proportion and stirring until the alkoxysilane is evenly dispersed in the alkoxysilane to form a translucent mixed liquid a; adding an aqueous polyester resin dispersion and deionized water to the nano-silicon dioxide aqueous dispersion and stirring evenly to obtain a mixed liquid b; slowly dropping the mixed liquid a into the mixed liquid b for 25 minutes, then heating to 40-65° C., reacting at a constant temperature for 4 hours, stopping heating and cooling to room temperature to obtain an aqueous nano-modified dispersion c;
[0104] (II) mixing the aqueous nano-modified dispersion c prepared in (I) with a pigment, a wetting dispersant, a defoaming agent, a leveling agent and part of deionized water, dispersing the mixture with a high-speed disperser for 10-30 min, and then grinding the mixture with a sand mill, controlling the temperature of the grinding base material to be below 63° C., adding a thickener and the remaining amount of deionized water after the fineness requirement is reached, and dispersing the mixture uniformly to obtain an aqueous modified inorganic nano-coating;
[0105] (III) Mixing anionic surfactant and water, and then slowly adding aminosilane to the aqueous solution of anionic surfactant for 20 minutes. After the addition is completed, continue to disperse for 2 hours, cool to room temperature, and obtain an aqueous silicone dispersion;
[0106] (IV) The water-based modified inorganic nano coating obtained in (II) is mixed with the water-based organosilicon dispersion obtained in (III), and the mixture is dispersed at a low speed for 30 minutes to obtain the topcoat.
[0107] Example 2
[0108] This embodiment provides a car wheel hub coating, comprising a powder coating layer, a primer layer, and a topcoat layer sequentially arranged on the surface of the car wheel hub.
[0109] The powder coating layer is formed by coating the powder coating on the surface of the automobile wheel hub; the powder coating is epoxy polyester powder coating.
[0110] The primer layer is formed by a primer; the primer comprises the following components in percentage by mass:
[0111] Water-based polyester resin (water-soluble polyester resin, Tongde 1PB83Y) 25%;
[0112] Water-based acrylic resin (water-soluble acrylic resin, Tongde 1AB911Y) 5%;
[0113] Water-based blocked isocyanate (Huiyu HY112) 15%;
[0114] Neutralizer (N,N-dimethylethanolamine) 1%;
[0115] Substrate wetting agent (polyether modified siloxane solution) 0.3%;
[0116] Leveling agent (BYK-346) 0.3%
[0117] Defoamer (BYK-011) 0.5%;
[0118] Thickener (Borchi Gel 0620) 0.8%;
[0119] Cosolvent (mixture of 50wt% ethylene glycol butyl ether and 50wt% ethanol) 5%;
[0120] Deionized water balance.
[0121] The topcoat layer is formed by a topcoat, and the topcoat includes the following components in percentage by mass:
[0122] Water-based modified inorganic nano coating 85%;
[0123] Aqueous organosilane dispersion 8%;
[0124] Deionized water balance.
[0125] in:
[0126] The aqueous organosilane dispersion comprises the following components in percentage by mass:
[0127] Aminosilane (3-aminopropyltrimethoxysilane) 60%;
[0128] Anionic surfactant (carboxylate type anionic surfactant) 3%,
[0129] Deionized water balance.
[0130] The water-based modified inorganic nano coating comprises the following components in percentage by mass:
[0131] Aqueous nano-modified dispersion 75%;
[0132] Pigment (titanium dioxide) 10%;
[0133] Wetting and dispersing agent 2%;
[0134] Leveling agent (BYK-346) 1%;
[0135] Defoamer (BYK-028) 0.5%;
[0136] Thickener (Borchi Gel 0620) 0.5%;
[0137] Deionized water balance.
[0138] Wherein: the aqueous nano-modified dispersion comprises the following components in percentage by mass:
[0139] Nano-silicon dioxide aqueous dispersion (solid content 35%, average particle size 80nm, pH value 8) 40%;
[0140] Alkoxysilane (methyltrimethoxysilane) 30%,
[0141] Water-based polyester dispersion (Tongde 3PB811W) 15%,
[0142] Anionic surfactant (carboxylate type anionic surfactant) 3%,
[0143] Deionized water balance.
[0144] The preparation method of the automobile wheel hub coating of this embodiment is the same as that of Example 1.
[0145] Example 3
[0146] This embodiment provides a car wheel hub coating, comprising a powder coating layer, a primer layer, and a topcoat layer sequentially arranged on the surface of the car wheel hub.
[0147] The powder coating layer is formed by coating the powder coating on the surface of the automobile wheel hub; the powder coating is epoxy polyester powder coating.
[0148] The primer layer is formed by a primer; the primer comprises the following components in percentage by mass:
[0149] Water-based polyester resin (water-soluble polyester resin, Tongde 1PB83Y) 20%;
[0150] Water-based acrylic resin (water-soluble acrylic resin, Tongde 1AB911Y) 10%;
[0151] Water-based blocked isocyanate (HDI, Huiyu HY112) 5%;
[0152] Neutralizer (N,N-dimethylethanolamine) 1%;
[0153] Substrate wetting agent (polyether modified siloxane solution) 0.3%;
[0154] Leveling agent (BYK-346) 0.3%
[0155] Defoamer (BYK-011) 0.5%;
[0156] Thickener (Borchi Gel 0620) 0.8%;
[0157] Cosolvent (mixture of 50wt% ethylene glycol butyl ether and 50wt% ethanol) 5%;
[0158] Deionized water balance.
[0159] The topcoat layer is formed by a topcoat, and the topcoat includes the following components in percentage by mass:
[0160] Water-based modified inorganic nano coating 93%;
[0161] Aqueous organosilane dispersion 5%;
[0162] Deionized water balance.
[0163] in:
[0164] The aqueous organosilane dispersion comprises the following components in percentage by mass:
[0165] Aminosilane (3-aminopropyltrimethoxysilane) 55%;
[0166] Anionic surfactant (carboxylate type anionic surfactant) 2%,
[0167] Deionized water balance.
[0168] The water-based modified inorganic nano coating comprises the following components in percentage by mass:
[0169] Aqueous nano-modified dispersion 55%;
[0170] Pigment (titanium dioxide) 25%;
[0171] Wetting and dispersing agent 2%;
[0172] Leveling agent (BYK-346) 1%;
[0173] Defoamer (BYK-028) 0.5%;
[0174] Thickener (Borchi Gel 0620) 0.5%;
[0175] Deionized water balance.
[0176] Wherein: the aqueous nano-modified dispersion comprises the following components in percentage by mass:
[0177] Nano-silicon dioxide aqueous dispersion (solid content 25%, average particle size 110nm, pH 8) 50%; alkoxysilane (methyltrimethoxysilane) 25%,
[0178] Water-based polyester dispersion (Tongde 3PB811W) 20%,
[0179] Anionic surfactant (carboxylate type anionic surfactant) 3%,
[0180] Deionized water balance.
[0181] The preparation method of the automobile wheel hub coating of this embodiment is the same as that of Example 1.
[0182] Example 4
[0183] This embodiment provides a car wheel hub coating, comprising a powder coating layer, a primer layer, and a topcoat layer sequentially arranged on the surface of the car wheel hub.
[0184] The powder coating layer is formed by coating the powder coating on the surface of the automobile wheel hub; the powder coating is epoxy polyester powder coating.
[0185] The primer layer is formed of a primer; the primer is the same as the primer of Example 1.
[0186] The topcoat layer is formed by a topcoat, which is substantially the same as the topcoat of Example 1, except that the water-based nano-modified dispersion in the topcoat further comprises the following components in percentage by mass: 6% water-based acrylic resin microcapsules and 6% isocyanate microcapsules. That is, the water-based nano-modified dispersion in the topcoat of this embodiment comprises the following components in percentage by mass:
[0187] Nano-silicon dioxide aqueous dispersion (solid content 25%, average particle size 110nm, pH 8) 50%;
[0188] Alkoxysilane (methyltrimethoxysilane) 25%,
[0189] Water-based polyester dispersion (Tongde 3PB811W) 20%,
[0190] Water-based acrylic resin microcapsules (microcapsules obtained in Example 1 of CN107715811B) 6%,
[0191] Isocyanate microcapsules (microcapsules obtained in Example 1 of CN109535315B) 6%,
[0192] Anionic surfactant (carboxylate type anionic surfactant) 3%,
[0193] Deionized water balance.
[0194] The preparation method of the automobile wheel hub coating of this embodiment is basically the same as that of Example 1, except that in the preparation method of the topcoat of this embodiment, in step (I), an aqueous polyester resin dispersion, aqueous acrylic resin microcapsules, isocyanate microcapsules and deionized water are added to an aqueous nano-silicon dioxide dispersion and stirred evenly to obtain a mixed liquid b.
[0195] Example 5
[0196] This embodiment provides a car wheel hub coating, comprising a powder coating layer, a primer layer, and a topcoat layer sequentially arranged on the surface of the car wheel hub.
[0197] The powder coating layer is formed by coating the powder coating on the surface of the automobile wheel hub; the powder coating is epoxy polyester powder coating.
[0198] The primer layer is formed of a primer; the primer is the same as the primer of Example 1.
[0199] The topcoat layer is formed by a topcoat, which is substantially the same as the topcoat of Example 1, except that the water-based nano-modified dispersion in the topcoat further comprises the following components in mass percentages: 5% water-based acrylic resin microcapsules and 5% isocyanate microcapsules. That is, the water-based nano-modified dispersion in the topcoat of this embodiment comprises the following components in mass percentages:
[0200] Nano-silicon dioxide aqueous dispersion (solid content 25%, average particle size 110nm, pH 8) 50%;
[0201] Alkoxysilane (methyltrimethoxysilane) 25%,
[0202] Water-based polyester dispersion (Tongde 3PB811W) 20%,
[0203] Water-based acrylic resin microcapsules (microcapsules obtained in Example 1 of CN107715811B) 5%,
[0204] Isocyanate microcapsules (microcapsules obtained in Example 1 of CN109535315B) 5%,
[0205] Anionic surfactant (carboxylate type anionic surfactant) 3%,
[0206] Deionized water balance.
[0207] The preparation method of the automobile wheel hub coating of this embodiment is the same as that of Example 4.
[0208] Example 6
[0209] This embodiment provides a car wheel hub coating, comprising a powder coating layer, a primer layer, and a topcoat layer sequentially arranged on the surface of the car wheel hub.
[0210] The powder coating layer is formed by coating the powder coating on the surface of the automobile wheel hub; the powder coating is epoxy polyester powder coating.
[0211] The primer layer is formed of a primer; the primer is the same as the primer of Example 1.
[0212] The topcoat layer is formed by a topcoat, which is substantially the same as the topcoat of Example 1, except that the water-based nano-modified dispersion in the topcoat further comprises the following components in percentage by mass: 8% water-based acrylic resin microcapsules and 8% isocyanate microcapsules. That is, the water-based nano-modified dispersion in the topcoat of this embodiment comprises the following components in percentage by mass:
[0213] Nano-silicon dioxide aqueous dispersion (solid content 25%, average particle size 110nm, pH 8) 50%;
[0214] Alkoxysilane (methyltrimethoxysilane) 25%,
[0215] Water-based polyester dispersion (Tongde 3PB811W) 20%,
[0216] Water-based acrylic resin microcapsules (microcapsules obtained in Example 1 of CN109535315B) 8%,
[0217] Isocyanate microcapsules (microcapsules obtained in Example 1 of CN109535315B) 8%,
[0218] Anionic surfactant (carboxylate type anionic surfactant) 3%,
[0219] Deionized water balance.
[0220] The preparation method of the automobile wheel hub coating of this embodiment is the same as that of Example 4.
[0221] Example 7
[0222] This embodiment provides an application of an automobile wheel hub coating on the surface of an automobile aluminum alloy wheel hub.
[0223] The automobile wheel hub coatings of Examples 1-6 were respectively applied to A356 series cast automobile aluminum alloy wheel hubs.
[0224] Before spraying powder coating on the surface of A356 series cast aluminum alloy wheels, the cast and processed aluminum alloy wheels are subjected to chrome-free pretreatment and then coated with powder coating.
[0225] Table 1 Primer raw material components and mass percentage (100%)
[0226]
[0227] Table 2 Raw material components and mass percentage of topcoat (100%)
[0228]
[0229] Table 3 Raw material components and mass percentages of water-based modified inorganic nano coatings (100%)
[0230]
[0231] Table 4 Raw material components and mass percentages of aqueous nano-modified dispersions (100%) Table 5 Raw material components and mass percentages of aqueous silicone dispersion (100%)
[0232]
[0233] The automobile wheel hub coatings obtained in the above Examples 1-6 were tested respectively. The test results are shown in the following table. Comparative Example 1 is an organic coating of primer-color paint-clear varnish sprayed on the surface of an existing automobile wheel hub.
[0234] Table 6 Automobile wheel hub coating test results
[0235]
[0236]
[0237] Wherein: *The detection method of coating repair efficiency is: using a knife to make a cross on the surface of the coating to damage the automobile wheel hub coating of Examples 4-6 respectively, so as to make it self-repair, and after 7 days of self-repair, the scratch repair rate and coating adhesion are tested.
[0238] From the test results in Table 6, it can be seen that the automobile wheel hub coatings provided in Examples 1-6 of the present invention have good hardness, adhesion, neutral salt spray resistance, aging resistance, wear resistance, and impact resistance. After adding isocyanate microcapsules and water-based acrylic resin microcapsules to Examples 4-6 of the present invention, they have self-repairing functions, and the self-repairing rate is as high as ≥90%, and the adhesion of the repaired coatings is still good.
[0239] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and the present invention is also intended to include these modifications and modifications.
Claims
1. An automobile wheel hub coating, characterized in that: It includes a powder coating layer, a primer layer, and a topcoat layer which are sequentially arranged on the surface of the automobile wheel hub; The powder coating layer is formed by coating the powder coating on the surface of the automobile wheel hub; the powder coating is epoxy polyester powder coating; The primer layer is formed by a primer; the primer comprises the following components in mass percentage: 20-30% water-based polyester resin; 5-10% water-based acrylic resin; 5-15% water-based blocked isocyanate; 0.1-2.5% neutralizer; 0.1-0.5% substrate wetting agent; 0.1-0.5% leveling agent; 0.2-0.8% defoamer; 0.1-1.0% thickener; 2-6% cosolvent; the balance is deionized water; The topcoat layer is formed by a topcoat; the topcoat comprises the following components in percentage by mass: 85-95% of a water-based modified inorganic nano coating, 5-8% of a water-based organic silane dispersion, and the balance of deionized water; in: The water-based modified inorganic nano coating comprises the following components in percentage by mass: 55-75% of water-based modified nano dispersion, 5-25% of pigment, 0.2-3% of wetting dispersant, 0.5-2% of leveling agent, 0.1-0.8% of defoamer, 0.1-0.9% of thickener, and the balance of deionized water; The aqueous nano-modified dispersion comprises the following components in percentage by mass: 40-50% aqueous nano-silicon dioxide dispersion, 25-35% alkoxysilane, 10-30% aqueous polyester dispersion, 0.5-5% anionic surfactant, and the balance deionized water; The aqueous organic silane dispersion comprises the following components in percentage by mass: 45-65% aminosilane, 0.5-5% anionic surfactant, and the balance deionized water.
2. The automotive wheel hub coating according to claim 1, characterized in that: The aqueous nano-modified dispersion also includes the following components in percentage by mass: 5-8% aqueous acrylic resin microcapsules and 5-8% isocyanate microcapsules; the aqueous acrylic resin microcapsules include a first wall material and a first core material, the first wall material includes urea-formaldehyde resin, and the first core material includes aqueous acrylic resin; the isocyanate microcapsules include a second wall material and a second core material, the second wall material includes nano-silica, the second core material includes isocyanate, and the isocyanate is aqueous isocyanate.
3. The automotive wheel hub coating according to claim 1, characterized in that: In the primer, the water-based polyester resin is a water-soluble polyester resin, with a solid content of 60-80% and a hydroxyl content of 90-150 mgKOH / g, wherein the hydroxyl content is the hydroxyl content when converted to 100% resin solids; in the topcoat, the solid content of the water-based polyester dispersion is 30-50%, and the hydroxyl content is 60-120 mgKOH / g, wherein the hydroxyl content is the hydroxyl content when converted to 100% resin solids, and the pH value is 7.0-9.
0.
4. The automotive wheel hub coating according to claim 1, characterized in that: The nano-silicon dioxide aqueous dispersion has a solid content of 25-35%, an average particle size of 10-110 nm, and a pH value of 7-10.
5. The automotive wheel hub coating according to claim 1, characterized in that: The alkoxysilane is one of methyltrimethoxysilane and methyltriethoxysilane or a mixture of the two.
6. The automotive wheel hub coating according to claim 1, characterized in that: The water-based acrylic resin is a water-soluble acrylic resin with a solid content of 55-75% and a hydroxyl content of 60-90 mgKOH / g, wherein the hydroxyl content is the hydroxyl content when converted to 100% resin solid content.
7. The automotive wheel hub coating according to claim 1, characterized in that: The water-based blocked isocyanate is of HDI type, with a solid content of 65%-85%, an NCO content of 8-11%, and a deblocking temperature of 100-120°C.
8. A method for preparing an automobile wheel hub coating according to any one of claims 1 to 7, characterized in that: The invention comprises the following preparation methods: S1: spraying the powder coating on the surface of the automobile wheel hub and curing it at 160-200°C to form a powder coating layer with a thickness of 50-90 μm; S2: spraying primer and topcoat respectively on the surface of the powder coating layer obtained in S1, and curing at 120-130° C. to form a primer layer and a topcoat layer respectively, wherein the thickness of the primer layer is 3-8 μm, and the thickness of the topcoat layer is 15-30 μm; thereby obtaining the automobile wheel hub coating.
9. Use of the automobile wheel hub coating according to any one of claims 1 to 7 on the surface of an automobile aluminum alloy wheel hub.
10. The application of the automobile wheel hub coating according to claim 9 on the surface of an automobile aluminum alloy wheel hub is characterized in that: The automobile aluminum alloy wheel hub is an automobile aluminum alloy wheel hub cast in the A356 series.