A synergistic compound light stabilizer for automotive paint and its preparation method

By introducing cyanuric chloride and resorcin into the car paint, combined with a light stabilizer system of 1,6-hexanediamine piperidine, the problem of unstable performance caused by the small molecular weight of the existing light stabilizers was solved and achieved The long-lasting photostability and compatibility of car paint coatings slow down the photoaging process.

CN117363085BActive Publication Date: 2024-10-01ZHENXING FINE CHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311496370.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-10
Publication Date
2024-10-01
Estimated Expiration
2043-11-10

AI Technical Summary

Technical Problem

The hindered amine light stabilizers in existing car paints have problems such as small molecular weight, easy volatilization, easy migration and easy degradation, which affects their anti-aging effect. At the same time, large molecular weight affects the effective nitrogen content, resulting in unstable light stability performance.

Method used

A synergistic compound light stabilizer for car paint is used. By introducing cyanuric chloride and resorcinol, and adding 1,6-hexamethylenediamine piperidine to the triazine structure light stabilizer, the synthesized compound has good It has the function of UV absorption and free radical capture, and by adjusting the ratio of light stabilizers A and B, adding antioxidants and other additives to improve compatibility and stability.

Benefits of technology

It achieves balanced stability and anti-aging effects, maintains coating performance and color stability, expands the application scope of light stabilizers in car paints, and improves the yield and compatibility of synthetic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004542765580000021
    Figure BDA0004542765580000021
  • Figure BDA0004542765580000031
    Figure BDA0004542765580000031
  • Figure BDA0004542765580000091
    Figure BDA0004542765580000091
Patent Text Reader

Abstract

The present invention provides a synergistic composite light stabilizer for vehicle paint and a preparation method thereof, wherein the light stabilizer comprises the following raw materials in parts by weight: 20 to 50 parts of light stabilizer A, 4 to 40 parts of light stabilizer B, 2 to 10 parts of antioxidant, and 5 to 15 parts of other additives. The light stabilizer provided by the present invention has a suitable molecular weight, can effectively improve the light stability of vehicle paint, has good compatibility with vehicle paint, has a high product yield, and is suitable for industrialization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of light stabilizer preparation, and particularly relates to a synergistic compound light stabilizer for vehicle paint and a preparation method thereof. Background Art

[0002] Long-term exposure to light, heat, humidity and oxygen will cause light aging of the paint coating, among which light is the most important factor. In order to extend the service life of the coating, an appropriate amount of light stabilizer is usually added to the coating to delay the light aging process.

[0003] Among various types of additives, hindered amine light stabilizers (HALS) have attracted much attention due to their high light stabilization efficiency. HALS is a type of light stabilizer with excellent anti-aging properties, which can capture free radicals, decompose peroxides and quench singlet oxygen. Therefore, the application of HALS in car paint coatings can effectively extend the service life of the coating.

[0004] However, the commonly used hindered amine light stabilizers on the market have the problems of small molecular weight, easy volatility, easy migration and easy degradation, while the large molecular weight will affect the effective nitrogen content, thereby affecting the anti-aging effect. Therefore, it is very necessary to develop a hindered amine light stabilizer system that balances stability and anti-aging effects. Summary of the invention

[0005] In view of the defects of the prior art, the purpose of the present invention is to provide a synergistic compound light stabilizer for car paint and a preparation method thereof, which can effectively play the role of the light stabilizer and balance the stability and anti-aging effects; at the same time, it has good compatibility with the main component of car paint, acrylic resin, and still maintains coating performance and color stability after light aging.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] On one hand, the present invention provides a synergistic compound light stabilizer for vehicle paint, characterized in that the light stabilizer comprises the following raw materials in parts by weight: 20 to 50 parts of light stabilizer A, 4 to 40 parts of light stabilizer B, 2 to 10 parts of antioxidant and 5 to 15 parts of other additives;

[0008] The structural formula of the light stabilizer A is shown in formula (I):

[0009]

[0010] Preferably, the preparation steps of light stabilizer A are as follows:

[0011] (1) adding 2,2,6,6-tetramethylpiperidinamine, cyanuric chloride, organic solvent A and catalyst A into a reactor, reacting at 50-80° C. for 6-18 hours, washing, filtering and drying to obtain a solid, namely intermediate I;

[0012] (2) adding intermediate I, 1,6-hexanediaminepiperidine, organic solvent B and catalyst B into a reactor, reacting at 60-80° C. for 4-12 hours, washing, filtering and drying to obtain a solid, namely intermediate II;

[0013] (3) Add intermediate II, resorcinol, organic solvent C and catalyst C into a reactor, react at 40-60° C. for 4-10 hours, and obtain light stabilizer A after washing, filtering and drying.

[0014] Further preferably, the preparation reaction of the light stabilizer A is as follows:

[0015]

[0016] The applicant introduced cyanuric chloride and resorcinol, and added 1,6-hexanediaminepiperidine prepolymer to a triazine-structured light stabilizer, so that the synthesized compound has good ultraviolet absorption ability and the function of capturing free radicals and quenching singlet oxygen, solving the problem of unstable light stability caused by the single function and small molecular weight of general light stabilizers; at the same time, the introduction of the hydrophilic group phenolic hydroxyl group modified the main functional body of the light stabilizer, so that the synthesized compound has good solubility properties, making it more widely used in car paint coatings.

[0017] Preferably, in the preparation step (1), the molar ratio of 2,2,6,6-tetramethylpiperidinamine to cyanuric chloride is (1-1.5):1.

[0018] Preferably, the molar ratio of intermediate I to 1,6-hexanediaminepiperidine in the preparation step (2) is (2.5-3):1.

[0019] Preferably, the molar ratio of intermediate II to resorcinol in the preparation step (3) is 1:(1.8-2.5).

[0020] Further preferably, the amount of the organic solvent A added is 10 to 20 times that of 2,2,6,6-tetramethylpiperidinamine;

[0021] More preferably, the organic solvent A is toluene.

[0022] Further preferably, the amount of the organic solvent B added is 10 to 18 times that of the intermediate I;

[0023] More preferably, the organic solvent B is m-xylene.

[0024] Further preferably, the amount of the organic solvent C added is 8 to 15 times that of the intermediate II;

[0025] More preferably, the organic solvent C is methanol.

[0026] Preferably, in the preparation step (1), the catalyst A is 15 wt% sodium hydroxide;

[0027] More preferably, the molar ratio of the sodium hydroxide to 2,2,6,6-tetramethylpiperidinamine is (1-1.2):1.

[0028] Preferably, in the preparation step (2), the catalyst B is anhydrous aluminum chloride;

[0029] More preferably, the molar ratio of the anhydrous aluminum chloride to the intermediate I is (1.2-1.4):1.

[0030] Preferably, in the preparation step (3), the catalyst C is 20 wt% of sodium hydroxide;

[0031] More preferably, the molar ratio of the sodium hydroxide to the intermediate II is (1.3-1.5):1.

[0032] Preferably, an inorganic base is also added in the preparation step (3);

[0033] The molar ratio of the inorganic base to the intermediate II is (0.5-0.8):1.

[0034] More preferably, the inorganic base is at least one of sodium carbonate and potassium carbonate.

[0035] The applicant found that during the synthesis process, the addition of a medium-strong alkaline inorganic base can effectively increase the product yield. This may be because, compared with a strong base, the inorganic base avoids the reaction of the phenolic hydroxyl group and reduces the reaction of the by-products; however, when a weak base is added, the reaction is not thorough, and there is excess raw material in the synthesis system, which is not conducive to improving the yield.

[0036] Preferably, the light stabilizer B is light stabilizer 944;

[0037] The mass ratio of the light stabilizer B to the light stabilizer A is (0.5-1.5):1.

[0038] More preferably, the mass ratio of the light stabilizer B to the light stabilizer A is 1:1.

[0039] The applicant also added light stabilizer B and light stabilizer A for compound use. The applicant found that by adjusting the ratio between the two light stabilizers, it is beneficial to improve the compatibility of the light stabilizers in the car paint coating. Light stabilizer B showed better synergistic effect in the system, greatly improved the stabilizing effect of the light stabilizer, and at the same time delayed the changes in the optical properties of the car paint coating, such as fading.

[0040] Preferably, the antioxidant is at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and tris[2,4-di-tert-butylphenyl]phosphite;

[0041] Further preferably, the antioxidant is tris[2,4-di-tert-butylphenyl]phosphite. Tris[2,4-di-tert-butylphenyl]phosphite antioxidant can decompose highly active hydroperoxides into low-activity molecules. The applicant has found that adding it to the system can also have a synergistic effect on the anti-aging effect of the light stabilizer.

[0042] Preferably, the other additive is an organic solvent D;

[0043] Further preferably, the organic solvent D is at least one of toluene, xylene and ethyl acetate.

[0044] Preferably, the light stabilizer further contains 1 to 3 parts by weight of an optical brightener;

[0045] Further preferably, the optical brightener is brightener RQT-A-1.

[0046] On the other hand, the present invention provides a method for preparing a synergistic compound light stabilizer for vehicle paint, which is characterized in that it comprises the following steps: mixing the light stabilizer A, light stabilizer B, antioxidant and other additives according to proportion under nitrogen protection, heating and stirring at 60-70° C., reacting for 5-10 hours, filtering, separating and purifying to obtain the synergistic compound light stabilizer for vehicle paint.

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] (1) The synergistic composite light stabilizer for vehicle paint provided by the present invention introduces cyanuric chloride and resorcinol, and adds 1,6-hexanediaminepiperidine to carry out prepolymerization on the basis of a light stabilizer with a triazine structure, so that the synthesized compound has good ultraviolet absorption ability and the function of capturing free radicals and quenching singlet oxygen, thereby solving the problem of unstable light stability performance caused by the single function and small molecular weight of general light stabilizers.

[0049] (2) The synergistic composite light stabilizer for vehicle paint provided by the present invention modifies the main functional body of the light stabilizer by introducing a hydrophilic group phenolic hydroxyl group, so that the synthesized compound has good solubility, thereby making it more widely used in vehicle paint coatings.

[0050] (3) The synergistic composite light stabilizer for vehicle paint provided by the present invention avoids the reaction of phenolic hydroxyl groups and reduces the generation of by-products by adding a medium-strong alkaline inorganic base; at the same time, it avoids the problem of residual raw materials in the system due to incomplete reaction, and effectively improves the yield of the synthetic product.

[0051] (4) The synergistic compound light stabilizer for vehicle paint provided by the present invention is an excellent composite stabilizer. By compounding light stabilizer A and light stabilizer B in a mass ratio of (0.5-1.5):1, light stabilizer B exhibits a better synergistic effect in the system, which is beneficial to improving the compatibility of the light stabilizer in the vehicle paint coating and greatly improving the stabilizing effect of the light stabilizer. DETAILED DESCRIPTION

[0052] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0053] Unless otherwise specified, the reagents used in the examples can be easily obtained from commercial companies.

[0054] Example 1

[0055] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 35 parts of light stabilizer A, 35 parts of light stabilizer B, 7 parts of antioxidant, 10 parts of other additives and 2.5 parts of optical brightener.

[0056] The preparation reaction of the light stabilizer A in this embodiment is as follows:

[0057] (1) 120 mmol 2,2,6,6-tetramethylpiperidinamine, 100 mmol cyanuric chloride, 172 mL toluene and 132 mmol sodium hydroxide were added to a reactor, reacted at 70° C. for 12 h, and washed, filtered and dried to obtain a solid, namely, intermediate I;

[0058] (2) 270 mmol of intermediate I, 100 mmol of 1,6-hexanediaminepiperidine, 496 mL of m-xylene and 351 mmol of anhydrous aluminum chloride were added to a reactor, reacted at 70° C. for 8 h, and solid intermediate II was obtained after washing, filtering and drying;

[0059] (3) 50 mmol of intermediate II, 105 mmol of resorcinol, 25 mL of methanol and 70 mmol of sodium hydroxide were added to a reactor, reacted at 55° C. for 7 h, and washed, filtered and dried to obtain light stabilizer A. 4.83 g of potassium carbonate was also added in the preparation step (3). The preparation reaction obtained 5.84 g of the light stabilizer A, with a yield of 95.7%.

[0060] Light stabilizer A was dissolved in methanol in a centrifuge tube and then tested by LC-MS. The mass spectrum data (m / z) obtained were as follows: 1062.76 (100%), 1063.76 (70.2%), 1080.50 (4.4%). The theoretical value was basically consistent with the actual measured value.

[0061] The preparation steps of the synergistic composite light stabilizer for vehicle paint in this embodiment include: mixing the light stabilizer A, light stabilizer B, antioxidant and other additives in proportion under nitrogen protection, heating and stirring at 65° C., reacting for 7.5 hours, filtering, separating and purifying to obtain the synergistic composite light stabilizer for vehicle paint. The light stabilizer B is light stabilizer 944, the antioxidant is tris[2,4-di-tert-butylphenyl]phosphite, the other additives are toluene, and the optical brightener is brightener RQT-A-1.

[0062] Example 2

[0063] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 20 parts of light stabilizer A, 40 parts of light stabilizer B, 2 parts of antioxidant, 5 parts of other additives and 1 part of optical brightener.

[0064] The preparation reaction of the light stabilizer A in this example is the same as that in Example 1.

[0065] In step (1), 100 mmol 2,2,6,6-tetramethylpiperidinamine, 100 mmol cyanuric chloride, 106 mL toluene and 100 mmol sodium hydroxide were added; in step (2), 250 mmol intermediate I, 100 mmol 1,6-hexanediamine piperidine, 308 mL m-xylene and 300 mmol anhydrous aluminum chloride were added; in step (3), 50 mmol intermediate II, 90 mmol resorcinol, 16 mL methanol and 65 mmol sodium hydroxide were added. In preparation step (3), 3.45 g potassium carbonate was also added. The preparation reaction obtained 5.80 g of the light stabilizer A, with a yield of 95.1%.

[0066] The preparation steps of the synergistic composite light stabilizer for vehicle paint in this embodiment include: mixing the light stabilizer A, light stabilizer B, antioxidant and other additives in proportion under nitrogen protection, heating and stirring at 60° C., reacting for 10 hours, filtering, separating and purifying to obtain the synergistic composite light stabilizer for vehicle paint. The light stabilizer B is light stabilizer 944, the antioxidant is tris[2,4-di-tert-butylphenyl]phosphite, the other additives are toluene, and the optical brightener is brightener RQT-A-1.

[0067] Example 3

[0068] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 50 parts of light stabilizer A, 4 parts of light stabilizer B, 10 parts of antioxidant, 15 parts of other additives and 4 parts of optical brightener.

[0069] The preparation reaction of the light stabilizer A in this example is the same as that in Example 1.

[0070] In step (1), 150 mmol 2,2,6,6-tetramethylpiperidinamine, 100 mmol cyanuric chloride, 319 mL toluene and 180 mmol sodium hydroxide were added; in step (2), 300 mmol intermediate I, 100 mmol 1,6-hexanediamine piperidine, 666 mL m-xylene and 420 mmol anhydrous aluminum chloride were added; in step (3), 50 mmol intermediate II, 125 mmol resorcinol, 30 mL methanol and 75 mmol sodium hydroxide were added. In preparation step (3), 5.52 g potassium carbonate was also added. The preparation reaction obtained 5.82 g of the light stabilizer A, with a yield of 95.4%.

[0071] The preparation steps of the synergistic composite light stabilizer for vehicle paint in this embodiment include: mixing the light stabilizer A, light stabilizer B, antioxidant and other additives in proportion under nitrogen protection, heating and stirring at 70° C., reacting for 5 hours, filtering, separating and purifying to obtain the synergistic composite light stabilizer for vehicle paint. The light stabilizer B is light stabilizer 944, the antioxidant is tris[2,4-di-tert-butylphenyl]phosphite, the other additives are toluene, and the optical brightener is brightener RQT-A-1.

[0072] Example 4

[0073] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 10 parts of light stabilizer A, 5 parts of light stabilizer B, 2 parts of antioxidant, 5 parts of other additives and 1 part of optical brightener.

[0074] The preparation reaction of the light stabilizer A in this example is the same as that in Example 1.

[0075] The preparation steps of the synergistic compound light stabilizer for vehicle paint in this embodiment are the same as those in Example 1.

[0076] Example 5

[0077] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 20 parts of light stabilizer A, 30 parts of light stabilizer B, 10 parts of antioxidant, 15 parts of other additives and 2.5 parts of optical brightener.

[0078] The preparation reaction of the light stabilizer A in this example is the same as that in Example 1.

[0079] The preparation steps of the synergistic compound light stabilizer for vehicle paint in this embodiment are the same as those in Example 1.

[0080] Example 6

[0081] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 35 parts of light stabilizer A, 35 parts of light stabilizer B, 7 parts of antioxidant, and 10 parts of other additives.

[0082] The preparation reaction of the light stabilizer A in this example is the same as that in Example 1.

[0083] The preparation steps of the synergistic compound light stabilizer for vehicle paint in this embodiment are the same as those in Example 1.

[0084] Example 7

[0085] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 20 parts of light stabilizer A, 30 parts of light stabilizer B, 7 parts of antioxidant, 10 parts of other additives and 4.5 parts of optical brightener.

[0086] The preparation reaction of the light stabilizer A in this example is the same as that in Example 1.

[0087] The preparation steps of the synergistic compound light stabilizer for vehicle paint in this embodiment are the same as those in Example 1.

[0088] Example 8

[0089] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 35 parts of light stabilizer A, 35 parts of light stabilizer B, 7 parts of antioxidant, 10 parts of other additives and 2.5 parts of optical brightener.

[0090] The preparation reaction of the light stabilizer A in this example is the same as that in Example 1 except that the inorganic base is potassium bicarbonate. The preparation reaction obtains 5.47 g of the light stabilizer A with a yield of 89.7%.

[0091] The preparation steps of the synergistic compound light stabilizer for vehicle paint in this embodiment are the same as those in Example 1.

[0092] Example 9

[0093] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 35 parts of light stabilizer A, 35 parts of light stabilizer B, 7 parts of antioxidant, 10 parts of other additives and 2.5 parts of optical brightener.

[0094] The preparation reaction of the light stabilizer A in this example is the same as that in Example 1 except that the inorganic base is potassium hydroxide. The preparation reaction obtains 4.28 g of the light stabilizer A with a yield of 70.1%.

[0095] The preparation steps of the synergistic compound light stabilizer for vehicle paint in this embodiment are the same as those in Example 1.

[0096] Example 10

[0097] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 35 parts of light stabilizer A, 7 parts of antioxidant, 10 parts of other additives and 2.5 parts of optical brightener.

[0098] The preparation reaction of the light stabilizer A in this example is the same as that in Example 1.

[0099] The preparation steps of the synergistic compound light stabilizer for vehicle paint in this embodiment are the same as those in Example 1.

[0100] Embodiment 11

[0101] In the preparation reaction step (1) of the light stabilizer A in this example, the molar ratio of 2,2,6,6-tetramethylpiperidinamine to cyanuric chloride is 0.7:1, and the rest is consistent with Example 1.

[0102] Example 12

[0103] In the preparation reaction step (1) of the light stabilizer A in this example, the molar ratio of 2,2,6,6-tetramethylpiperidinamine to cyanuric chloride is 1.6:1, and the rest is consistent with Example 1.

[0104] Embodiment 13

[0105] In this example, except that the amount of potassium carbonate added in step (3) of preparing light stabilizer A is 4.14 g, the rest is consistent with Example 1. The preparation reaction obtains 5.76 g of light stabilizer A with a yield of 94.4%.

[0106] Embodiment 14

[0107] In this example, except that the amount of potassium carbonate added in step (3) of preparing light stabilizer A is 10.35 g, the rest is consistent with Example 1. The preparation reaction obtains 5.64 g of light stabilizer A with a yield of 92.5%.

[0108] Comparative Example 1

[0109] A synergistic compound light stabilizer for vehicle paint comprises the following raw materials in parts by weight: 35 parts of light stabilizer C, 35 parts of light stabilizer B, 7 parts of antioxidant, 10 parts of other additives and 2.5 parts of optical brightener.

[0110] The light stabilizer C in this embodiment is light stabilizer 119.

[0111] The preparation steps of the synergistic compound light stabilizer for vehicle paint in this embodiment are the same as those in Example 1.

[0112] Performance Testing:

[0113] (1) Photostability

[0114] The light stabilizer prepared in the example was added into the car paint at 0.6 wt %. The light stability performance test was characterized by the decomposition rate. According to GB / T16422.2-1999, a 24-hour light stability performance test was carried out.

[0115] (2) Color difference

[0116] The light stabilizer prepared in the example was added to the car paint at 0.6 wt %, and the paint was aged for 800 h using a xenon lamp according to ISO4892-3:2016 to detect the color difference change.

[0117] The specific test results are shown in Table 1.

[0118] Table 1

[0119]

[0120]

[0121] As can be seen from Table 1 above, the light stabilizer provided by the present invention can effectively play the role of light stabilizer, balance stability and anti-aging effects; at the same time, it has good compatibility with the main component of car paint acrylic resin, and the coating performance and color stability are still maintained after light aging. Among them, by comparing Examples 1-5 with Comparative Example 1, it can be seen that the synergistic compound light stabilizer provided by the present invention can effectively play the light stabilization effect of the light stabilizer in the car paint coating; by comparing Examples 1-5 with Examples 6 and 7, it can be seen that the light stabilizer provided by the present invention can maintain the gloss of the car paint and coordinate the color uniformity by adding a suitable amount of optical brightener; by comparing Examples 1-5 with Examples 8, 9 and Examples 13, 14, it can be seen that the light stabilizer provided by the present invention has some relatively obvious high yields when synthesizing light stabilizer A, which is suitable for efficient industrialization; by comparing Examples 1-9 with Example 10, it can be seen that the light stabilizer provided by the present invention has higher compatibility with car paint.

[0122] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A synergistic composite light stabilizer for vehicle paint, characterized in that: The light stabilizer comprises the following raw materials in parts by weight: 20-50 parts of light stabilizer A, 4-40 parts of light stabilizer B, 2-10 parts of antioxidant and 5-15 parts of other additives; The structural formula of the light stabilizer A is shown in formula (I): Formula (I); The light stabilizer B is light stabilizer 944.

2. The synergistic composite light stabilizer for vehicle paint according to claim 1, characterized in that: The preparation steps of the light stabilizer A are as follows: (1) Add 2,2,6,6-tetramethylpiperidinamine, cyanuric chloride, organic solvent A and catalyst A into a reactor, react at 50-80°C for 6-18 hours, and wash, filter and dry to obtain a solid, namely intermediate I; (2) Add intermediate I, 1,6-hexanediaminepiperidine, organic solvent B and catalyst B into a reactor, react at 60-80°C for 4-12 hours, and wash, filter and dry to obtain a solid, namely intermediate II; (3) Add intermediate II, resorcinol, organic solvent C and catalyst C into a reactor, react at 40-60°C for 4-10 hours, and obtain light stabilizer A after washing, filtering and drying.

3. The synergistic composite light stabilizer for vehicle paint according to claim 2, characterized in that: In the preparation step (1), the molar ratio of 2,2,6,6-tetramethylpiperidinamine to cyanuric chloride is (1-1.5):

1.

4. The synergistic composite light stabilizer for vehicle paint according to claim 2, characterized in that: In the preparation step, the organic solvents A, B and C are respectively at least one of methanol, sodium acetate, toluene and m-xylene; and the catalysts A, B and C are respectively at least one of 10-30wt% sodium hydroxide and anhydrous aluminum chloride.

5. The synergistic composite light stabilizer for vehicle paint according to claim 2, characterized in that: In the preparation step (3), an inorganic base is also added; The molar ratio of the inorganic base to the intermediate II is (0.5-0.8):

1.

6. The synergistic composite light stabilizer for vehicle paint according to claim 1, characterized in that: The mass ratio of the light stabilizer B to the light stabilizer A is (0.5-1.5):

1.

7. The synergistic composite light stabilizer for vehicle paint according to claim 1, characterized in that: The antioxidant is at least one of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester and tris[2,4-di-tert-butylphenyl]phosphite.

8. The synergistic composite light stabilizer for vehicle paint according to claim 1, characterized in that: The other additive is an organic solvent D.

9. The synergistic composite light stabilizer for vehicle paint according to claim 1, characterized in that: The light stabilizer also contains 1 to 4 parts by weight of an optical brightener.

10. The method for preparing the synergistic composite light stabilizer for vehicle paint according to any one of claims 1 to 9, characterized in that: The following steps are involved: The light stabilizer A, light stabilizer B, antioxidant and other additives are mixed according to proportion under nitrogen protection, heated at 60-70° C. with stirring, reacted for 5-10 hours, filtered, separated and purified to obtain the synergistic composite light stabilizer for vehicle paint.

Citation Information

Patent Citations

  • Low-alkalinity polymeric hindered amine light stabilizing agent and preparation method thereof

    CN105348525A

  • Novel triazine compound, composition and preparation method thereof

    CN109651275A

  • Method for preparing light stabilizer 2020 by skeleton method

    CN114853733A

  • Tetramethylpiperidine-based light stabilizer and preparation method thereof

    CN115895034A

  • Tetramethylpiperidyl-containing polysiloxane or polyamine / cyanuric cl / tetramethyl-4-piperidylamine stabilizer

    US6328912B1