A para-aramid fiber resistant to ultraviolet light and intelligent color change, and preparation method and application thereof
Through the composite modification treatment of DAE and PANI with para-aramid fiber, hydrogen bonds and reversible ultraviolet absorption capabilities are formed, which solves the problems of poor ultraviolet radiation resistance and insufficient mechanical properties of aramid 1414 fiber, and achieves ultraviolet aging resistance and The improvement of anti-fatigue performance is suitable for various industrial fields.
Patent Information
- Application Number
- CN202411017590.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Aramid 1414 fiber has problems such as low compressive strength, poor UV radiation resistance and weak surface and resin bonding force, which leads to a decrease in mechanical properties under long-term exposure to light, becoming brittle, cracked and yellowed, or even completely destroyed, affecting Its safe to use.
DAE and PANI are used for composite modification treatment with para-aramid fiber. By modifying para-aramid fiber in an organic solution, hydrogen bonding is formed to enhance its UV aging resistance, and it is provided through the synergy of DAE and PANI. Reversible UV absorption capability.
It improves the UV aging resistance and mechanical properties of para-aramid fiber, maintains good fatigue resistance, and simplifies the preparation process. It is suitable for smart wear, aerospace, automotive industry, sports equipment and other fields.
Smart Images

Figure CN118531632B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a para-aramid fiber resistant to ultraviolet light and intelligent color change, a preparation method and an application thereof, and belongs to the technical field of para-aramid fibers. Background Art
[0002] Aramid fiber is the general name for fully aromatic polyamide fibers. It can be divided into aramid I, aramid II and aramid III according to the types of synthetic monomers. It can also be named aramid 14, aramid 1313, aramid 1414, etc. according to the difference in the connection positions of the carbonyl and imine groups in the amide bond on the benzene ring. Polyparaphenylene terephthalamide (PPTA), also known as aramid 1414, is the most widely used aramid fiber and is often called para-aramid.
[0003] Aramid 1414 fiber itself has defects such as low compressive strength, poor UV resistance, and weak surface bonding with resin. In addition to the intrinsic properties of the material itself, the impact of the external environment on the material performance cannot be ignored. For aramid 1414, it is mainly the light aging effect. The effect of ultraviolet rays can cause the para-aramid fiber material to degrade, age and deteriorate, resulting in a gradual decrease in the mechanical properties of the product, brittleness, cracking and yellowing, or even complete destruction and unusability. Therefore, the safe use of aramid 1414 under the long-term action of light has attracted widespread attention.
[0004] Chinese patent application CN114753154A discloses an anti-ultraviolet para-aramid fiber and a preparation method thereof and an anti-ultraviolet fabric. The anti-ultraviolet para-aramid fiber comprises a para-aramid fiber filament and a polyacrylonitrile coating coated on the outside of the para-aramid fiber filament. The present invention provides anti-ultraviolet function to the para-aramid by coating polyacrylonitrile on the para-aramid fiber, thereby reducing the sensitivity of the para-aramid product to ultraviolet rays and extending the service life of the para-aramid. This method of coating with other materials has a complicated preparation process and will limit the subsequent application of the para-aramid. Chinese patent application CN105085902A discloses a method for preparing anti-ultraviolet aging para-aramid, by adding nano-SiO2 to p-phenylenediamine and\or terephthaloyl chloride, and the para-aramid can be prepared by a one-step method of a screw extruder. The method of adding silica in the preparation process of the para-aramid requires the preparation process of the para-aramid to be adjusted, the preparation process is complicated, and other properties of the para-aramid will also be affected. Chinese patent application CN113355906A discloses a UV-resistant zinc-modified composite para-aramid fiber and its preparation method and application, which mainly increases the UV resistance of para-aramid by ZnO modification, because ZnO particles have strong UV absorption ability and are effective UV shielding agents. However, the use of ZnO to modify the para-aramid fiber will affect other properties of the para-aramid fiber, such as causing the strength of the para-aramid fiber to decrease, thereby affecting other application properties of the para-aramid fiber. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a para-aramid fiber with UV-resistant intelligent color change, a preparation method and an application thereof, so as to solve the problem that the aramid 1414 fiber has poor UV radiation aging resistance, and at the same time, the aramid 1414 fiber has good strength performance and a simple preparation process.
[0006] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing a para-aramid fiber with ultraviolet resistance and intelligent color change, the preparation method comprising:
[0007] S1, placing the clean para-aramid fiber in a DAE (diarylethene) organic solution for modification to obtain aramid fiber DAE-THFL;
[0008] S2, placing the aramid fiber DAE-THFL in a PANI (polyaniline) organic solution and controlling the reaction temperature. After the reaction is completed, washing and drying are performed to obtain the para-aramid fiber resistant to ultraviolet light and having intelligent color change.
[0009] Furthermore, the DAE organic solution is prepared by dissolving DAE in an organic solvent, and the PANI organic solution is prepared by dissolving PANI in an organic solvent, and the organic solvent is N-methylpyrrolidone or N,N-dimethylformamide.
[0010] Furthermore, the DAE is (1-(5-formyl-2-methylthiophen-3-yl), 2-(1-methyl-2-methyl-indol-3-yl)) perfluorocyclopentene.
[0011] Furthermore, the concentration of the DAE organic solution is 300-900 μM; the concentration of the PANI organic solution is 0.4-0.6 mg / mL.
[0012] Furthermore, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is (3-5) g: (40-60) mL: (80-120) mL.
[0013] Furthermore, the modification treatment conditions of step S1 are carried out under oscillation or ultrasonic conditions, the treatment temperature is 55-65° C., and the treatment time is 20-40 min.
[0014] Furthermore, in step S2, the reaction process is carried out under oscillation or ultrasonic conditions, the reaction temperature is 55-65° C., and the reaction time is 3-6 h.
[0015] The invention also discloses a para-aramid fiber resistant to ultraviolet rays and capable of intelligent color change. The para-aramid fiber resistant to ultraviolet rays and capable of intelligent color change is prepared by the preparation method of the invention.
[0016] The present invention also discloses an application of a para-aramid fiber resistant to ultraviolet rays and having intelligent color change, wherein the para-aramid fiber resistant to ultraviolet rays and having intelligent color change is applied in the fields of smart wearables, aerospace, automobile industry and sports equipment.
[0017] The beneficial effects of the present invention are:
[0018] The preparation method of the present invention increases the ultraviolet aging resistance of para-aramid fiber by composite modification of PANI and DAE with para-aramid fiber. In the preparation method of the present invention, by controlling the process conditions, a strong hydrogen bond is formed between PANI, DAE and para-aramid fiber, so that the para-aramid fiber has lasting ultraviolet aging resistance and at the same time the para-aramid fiber maintains good mechanical properties.
[0019] The preparation method of the present invention first uses DAE to treat the para-aramid fiber, and then uses PANI to treat it, so that the para-aramid fiber has better resistance to ultraviolet aging. At the same time, the para-aramid fiber has good reversibility in resistance to ultraviolet aging, because DAE itself has good light response and fatigue resistance to ultraviolet rays. When DAE is irradiated with ultraviolet rays, it will be converted into a closed-loop state. DAE will be converted into an open-loop state when heated or exposed to natural light in the closed-loop state, so that it can continue to absorb ultraviolet rays. Therefore, in the preparation process, it is prioritized to ensure that DAE and the para-aramid fiber form hydrogen bonds, so that the final para-aramid fiber has better resistance to ultraviolet aging.
[0020] The PANI molecule main chain contains a large number of conjugated P electrons. When exposed to strong light, the electrons in the valence band of polyaniline will be excited to the conduction band, and additional electron-hole pairs will appear. At the same time, the electrons or holes on the impurity energy level in the excitation band will change its conductivity. It has strong ultraviolet absorption ability and is an effective ultraviolet shielding agent. The amide bond between the PANI molecule and the para-aramid fiber can form a strong hydrogen bond force, which enhances the composite effect of the PANI molecule and the para-aramid fiber.
[0021] DAE molecules have strong ultraviolet absorption ability, and the molecular structure of DAE molecules will change after absorbing ultraviolet rays, and this change in molecular structure is reversible. Therefore, DAE molecules can continuously absorb ultraviolet rays and are long-term effective ultraviolet shielding agents; DAE molecules contain aldehyde groups, which can form strong hydrogen bonding forces with the amide bonds of PANI and para-aramid fibers respectively, thereby enhancing the ternary composite effect between DAE, PANI and para-aramid fibers. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a schematic diagram of the chemical structure of the para-aramid fiber with UV resistance and intelligent color change according to the present invention. DETAILED DESCRIPTION
[0023] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0025] A method for preparing a para-aramid fiber with ultraviolet resistance and intelligent color change, the preparation method comprising:
[0026] S1, placing clean para-aramid fiber in DAE organic solution for modification treatment to obtain aramid fiber DAE-THFL;
[0027] S2, placing the aramid fiber DAE-THFL in a PANI organic solution and controlling the reaction temperature, after the reaction is completed, washing and drying to obtain the ultraviolet resistant intelligent color-changing para-aramid fiber, the chemical structure of which is as follows Figure 1 shown.
[0028] Specifically, the DAE organic solution is prepared by dissolving DAE in an organic solvent, and the PANI organic solution is prepared by dissolving PANI in an organic solvent, and the organic solvent is N-methylpyrrolidone or N,N-dimethylformamide.
[0029] More specifically, the DAE used in the embodiment of the present invention is (1-(5-formyl-2-methylthiophen-3-yl), 2-(1-methyl-2-methyl-indol-3-yl)) perfluorocyclopentene (CASNO: 1400275-94-6).
[0030] More specifically, the PANI (polyaniline) used in the embodiments of the present invention is (C6H7N)n (article number: A84984; brand: Innochem) with a purity of 98%.
[0031] More specifically, the para-aramid fiber used in the embodiment of the present invention is aramid 1414 fiber.
[0032] Specifically, the concentration of the DAE organic solution is 300-900 μM; the concentration of the PANI organic solution is 0.4-0.6 mg / mL.
[0033] Specifically, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is (3-5) g: (40-60) mL: (80-120) mL.
[0034] Specifically, the modification treatment conditions of step S1 are carried out under oscillation or ultrasonic conditions, the treatment temperature is 55-65° C., and the treatment time is 20-40 min.
[0035] Specifically, in step S2, the reaction process is carried out under oscillation or ultrasonic conditions, the reaction temperature is 55-65° C., and the reaction time is 3-6 h.
[0036] Specifically, during the washing, distilled water and ethanol are used for washing in sequence; the drying temperature is 65-75°C.
[0037] More specifically, the drying is performed under an inert gas environment, and the inert gas used is nitrogen or helium.
[0038] More specifically, before the para-aramid fiber is modified, the para-aramid fiber is first deoiled. The specific treatment method is: the para-aramid fiber containing the oil agent is washed in distilled water and acetone in turn, and Soxhlet extraction is performed with ethyl acetate as the extraction solvent at 50°C for 24 hours, and then dried in a vacuum oven at 60°C for 8 hours to obtain clean para-aramid fiber.
[0039] The invention discloses an application of a para-aramid fiber resistant to ultraviolet light and capable of intelligent color change. The para-aramid fiber resistant to ultraviolet light and capable of intelligent color change is applied in the fields of intelligent wearables, aerospace, automobile industry and sports equipment.
[0040] Example 1
[0041] Preparation of para-aramid fiber with ultraviolet resistance and intelligent color change, the preparation method is as follows:
[0042] (1) Preparation of DAE organic solution: DAE was added to N-methylpyrrolidone and an organic solution of DAE with a concentration of 300 μM was obtained after ultrasonication.
[0043] Preparation of PANI organic solution: PANI was added into N-methylpyrrolidone and then ultrasonicated to obtain a PANI organic solution with a concentration of 0.5 mg / mL.
[0044] In this embodiment, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is 4 g:50 mL:100 mL.
[0045] (2) placing clean para-aramid fiber in DAE organic solution and ultrasonicating it at 60°C for 30 min to obtain aramid fiber DAE-THFL;
[0046] (3) The aramid fiber DAE-THFL was placed in a PANI organic solution and ultrasonicated at 60°C for 4 hours. The aramid fiber sample was then washed with distilled water and ethanol in turn to remove N-methylpyrrolidone and excess DAE and PANI. Finally, it was dried at 70°C for 2 hours in an inert environment to obtain the para-aramid fiber DAE-THFL-PANI-1 with UV-resistant intelligent color change.
[0047] Example 2
[0048] Preparation of para-aramid fiber with ultraviolet resistance and intelligent color change, the preparation method is as follows:
[0049] (1) Preparation of DAE organic solution: DAE was added to N-methylpyrrolidone and an organic solution with a concentration of 600 μM was obtained after ultrasonication.
[0050] Preparation of PANI organic solution: PANI was added into N-methylpyrrolidone and then ultrasonicated to obtain a PANI organic solution with a concentration of 0.5 mg / mL.
[0051] In this embodiment, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is 5 g:60 mL:120 mL.
[0052] (2) placing clean para-aramid fiber in DAE organic solution and ultrasonicating it at 65°C for 20 min to obtain aramid fiber DAE-THFL;
[0053] (3) The aramid fiber DAE-THFL was placed in a PANI organic solution and ultrasonicated at 65°C for 3 hours. The aramid fiber sample was then washed with distilled water and ethanol in turn to remove N-methylpyrrolidone and excess DAE and PANI. Finally, it was dried at 75°C in an inert environment for 2 hours to obtain the para-aramid fiber DAE-THFL-PANI-2 with UV-resistant intelligent color change.
[0054] Example 3
[0055] Preparation of para-aramid fiber with ultraviolet resistance and intelligent color change, the preparation method is as follows:
[0056] (1) Preparation of DAE organic solution: DAE was added to N-methylpyrrolidone and an organic solution with a concentration of 900 μM was obtained after ultrasonication.
[0057] Preparation of PANI organic solution: PANI was added into N-methylpyrrolidone and then ultrasonicated to obtain a PANI organic solution with a concentration of 0.5 mg / mL.
[0058] In this embodiment, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is 3 g:40 mL:80 mL.
[0059] (2) placing clean para-aramid fiber in DAE organic solution and ultrasonicating it at 55°C for 40 min to obtain aramid fiber DAE-THFL;
[0060] (3) The aramid fiber DAE-THFL was placed in a PANI organic solution and ultrasonicated at 55°C for 6 hours. The aramid fiber sample was then washed with distilled water and ethanol in turn to remove N-methylpyrrolidone and excess DAE and PANI. Finally, it was dried at 65°C in an inert environment for 3 hours to obtain the para-aramid fiber DAE-THFL-PANI-3 with UV-resistant intelligent color change.
[0061] Example 4
[0062] Preparation of para-aramid fiber with ultraviolet resistance and intelligent color change, the preparation method is as follows:
[0063] (1) Preparation of DAE organic solution: DAE was added to N,N-dimethylformamide, and an organic solution of DAE with a concentration of 400 μM was obtained after ultrasonic treatment;
[0064] Preparation of PANI organic solution: PANI was added into N,N-dimethylformamide, and a PANI organic solution with a concentration of 0.6 mg / mL was obtained after ultrasonic treatment.
[0065] In this embodiment, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is 4 g:60 mL:100 mL.
[0066] (2) placing clean para-aramid fiber in DAE organic solution and ultrasonicating it at 60°C for 30 min to obtain aramid fiber DAE-THFL;
[0067] (3) The aramid fiber DAE-THFL was placed in a PANI organic solution and shaken at 60°C for 5 hours. The aramid fiber sample was then washed with distilled water and ethanol to remove N,N-dimethylformamide and excess DAE and PANI. Finally, it was dried at 70°C for 2 hours to obtain the UV-resistant intelligent color-changing para-aramid fiber DAE-THFL-PANI-4.
[0068] Example 5
[0069] Preparation of para-aramid fiber with ultraviolet resistance and intelligent color change, the preparation method is as follows:
[0070] (1) Preparation of DAE organic solution: DAE was added to N,N-dimethylformamide, and an organic solution of DAE with a concentration of 600 μM was obtained after ultrasonic treatment;
[0071] Preparation of PANI organic solution: PANI was added into N,N-dimethylformamide, and a PANI organic solution with a concentration of 0.4 mg / mL was obtained after ultrasonic treatment.
[0072] In this embodiment, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is 4 g:50 mL:100 mL.
[0073] (2) placing clean para-aramid fiber in DAE organic solution, shaking at 60 °C for 40 min, to obtain aramid fiber DAE-THFL;
[0074] (3) The aramid fiber DAE-THFL was placed in a PANI organic solution and shaken at 60°C for 4 hours. The aramid fiber sample was then washed with distilled water and ethanol to remove N,N-dimethylformamide and excess DAE and PANI. Finally, it was dried at 70°C for 2 hours to obtain the UV-resistant intelligent color-changing para-aramid fiber DAE-THFL-PANI-5.
[0075] Comparative Example 1
[0076] The same method as in Example 1 was used to treat the para-aramid fiber, except that DAE was not used and only PANI was used to treat the para-aramid fiber. The specific preparation process is as follows:
[0077] (1) Preparation of PANI organic solution: PANI was added to N-methylpyrrolidone and an organic solution with a concentration of 0.5 mg / mL was obtained after ultrasonic treatment.
[0078] In this comparative example, the usage ratio of the para-aramid fiber and the PANI organic solution is 4 g:100 mL.
[0079] (2) The clean para-aramid fiber was placed in a PANI organic solution and ultrasonically treated at 60°C for 4 hours. The aramid fiber sample was then washed with distilled water and ethanol to remove N-methylpyrrolidone and excess PANI. Finally, it was dried at 70°C for 2 hours to obtain the treated para-aramid fiber THFL-PANI-1#.
[0080] Comparative Example 2
[0081] The para-aramid fiber was treated by the same method as in Example 1, except that PANI was not used and only DAE was used to treat the para-aramid fiber. The specific preparation process is as follows:
[0082] (1) Preparation of DAE organic solution: DAE was added to N-methylpyrrolidone and an organic solution of DAE with a concentration of 300 μM was obtained after ultrasonication.
[0083] In this comparative example, the usage ratio of the para-aramid fiber and the DAE organic solution is 4 g:50 mL.
[0084] (2) placing clean para-aramid fiber in DAE organic solution and ultrasonicating it at 60°C for 30 min to obtain aramid fiber DAE-THFL;
[0085] (3) The aramid fiber sample was washed with distilled water and ethanol in turn to remove N-methylpyrrolidone and excess DAE, and finally dried at 70 °C in an inert environment for 2 hours to obtain the treated para-aramid fiber DAE-THFL-2#.
[0086] Comparative Example 3
[0087] The same method as in Example 1 is used to treat the para-aramid fiber, except that the treatment order of DAE and PANI on the para-aramid fiber is changed. The specific preparation process is as follows:
[0088] (1) Preparation of DAE organic solution: DAE was added to N-methylpyrrolidone and an organic solution of DAE with a concentration of 300 μM was obtained after ultrasonication.
[0089] Preparation of PANI organic solution: PANI was added into N-methylpyrrolidone and then ultrasonicated to obtain a PANI organic solution with a concentration of 0.5 mg / mL.
[0090] In this comparative example, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is 4 g:50 mL:100 mL.
[0091] (2) placing the clean para-aramid fiber in a PANI organic solution and ultrasonicating it at 60 °C for 4 hours to obtain aramid fiber PANI-THFL;
[0092] (3) The aramid fiber PANI-THFL was placed in a DAE organic solution and ultrasonicated at 60°C for 30 min. The aramid fiber sample was then washed with distilled water and ethanol in turn to remove N-methylpyrrolidone and excess DAE and PANI. Finally, it was dried at 70°C in an inert environment for 2 hours to obtain the treated para-aramid fiber DAE-THFL-PANI-3#.
[0093] Comparative Example 4
[0094] The para-aramid fiber was treated by the same method as in Example 1, except that the concentration of the DAE organic solution was increased. The specific preparation process was as follows:
[0095] (1) Preparation of DAE organic solution: DAE was added to N-methylpyrrolidone and then ultrasonicated to obtain a DAE organic solution with a concentration of 1500 μM;
[0096] Preparation of PANI organic solution: PANI was added into N-methylpyrrolidone and then ultrasonicated to obtain a PANI organic solution with a concentration of 0.5 mg / mL.
[0097] In this comparative example, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is 4 g:50 mL:100 mL.
[0098] (2) placing clean para-aramid fiber in DAE organic solution and ultrasonicating it at 60°C for 30 min to obtain aramid fiber DAE-THFL;
[0099] (3) The aramid fiber DAE-THFL was placed in a PANI organic solution and ultrasonically treated at 60°C for 4 hours. The aramid fiber sample was then washed with distilled water and ethanol to remove N-methylpyrrolidone and excess DAE and PANI. Finally, it was dried at 70°C for 2 hours to obtain the treated para-aramid fiber DAE-THFL-PANI-4#.
[0100] Comparative Example 5
[0101] The para-aramid fiber is treated in the same manner as in Example 1, except that the temperature in step (2) is lowered. The specific preparation process is as follows:
[0102] (1) Preparation of DAE organic solution: DAE was added to N-methylpyrrolidone and an organic solution of DAE with a concentration of 300 μM was obtained after ultrasonication.
[0103] Preparation of PANI organic solution: PANI was added into N-methylpyrrolidone and then ultrasonicated to obtain a PANI organic solution with a concentration of 0.5 mg / mL.
[0104] In this comparative example, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is 4 g:50 mL:100 mL.
[0105] (2) placing the clean para-aramid fiber in a DAE organic solution and ultrasonicating it for 30 min at 25 °C to obtain aramid fiber DAE-THFL;
[0106] (3) The aramid fiber DAE-THFL was placed in a PANI organic solution and ultrasonically treated at 60°C for 4 hours. The aramid fiber sample was then washed with distilled water and ethanol to remove N-methylpyrrolidone and excess DAE and PANI. Finally, it was dried at 70°C for 2 hours to obtain the treated para-aramid fiber DAE-THFL-PANI-5#.
[0107] Comparative Example 6
[0108] The para-aramid fiber is treated in the same manner as in Example 1, except that the temperature in step (3) is lowered. The specific preparation process is as follows:
[0109] (1) Preparation of DAE organic solution: DAE was added to N-methylpyrrolidone and an organic solution of DAE with a concentration of 300 μM was obtained after ultrasonication.
[0110] Preparation of PANI organic solution: PANI was added into N-methylpyrrolidone and then ultrasonicated to obtain a PANI organic solution with a concentration of 0.5 mg / mL.
[0111] In this comparative example, the usage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is 4 g:50 mL:100 mL.
[0112] (2) placing clean para-aramid fiber in DAE organic solution and ultrasonicating it at 60°C for 30 min to obtain aramid fiber DAE-THFL;
[0113] (3) The aramid fiber DAE-THFL was placed in a PANI organic solution and ultrasonically treated at 25°C for 4 hours. The aramid fiber sample was then washed with distilled water and ethanol to remove N-methylpyrrolidone and excess DAE and PANI. Finally, it was dried at 70°C for 2 hours to obtain the treated para-aramid fiber DAE-THFL-PANI-6#.
[0114] Blank example
[0115] (1) Place clean para-aramid fiber in N-methylpyrrolidone and ultrasonicate for 4.5 h at 60 °C.
[0116] (2) The aramid fiber sample was washed with distilled water and ethanol in turn to remove N-methylpyrrolidone, and finally dried at 70°C in an inert environment for 2 hours to obtain the para-aramid fiber of the blank example.
[0117] The para-aramid fibers modified in the above embodiments, comparative examples and blank examples were evaluated for their UV aging resistance, wherein the UV aging resistance experimental conditions were:
[0118] The modified para-aramid fibers were stretched and fixed on a bracket and fully exposed to direct ultraviolet light in a UV light box (power 50 W), and the test was carried out under standard atmospheric temperature: 23℃±2℃, relative humidity: 50%±4%. The modulus retention rate, tensile strength retention rate and relative viscosity retention rate of the para-aramid fibers at different aging times were measured, and the specific results are shown in Tables 1 to 3.
[0119] Among them, the test method of modulus retention is: Instron universal material testing instrument 34SC-1 tests the modulus of the same group of composite materials (para-aramid fiber after modification) after ultraviolet irradiation for different time periods, and the modulus of the composite material (para-aramid fiber after modification) not irradiated with ultraviolet light is taken as 100%.
[0120] The test method for tensile strength retention is: Instron universal materials testing instrument 34SC-1 tests the strength of the same group of composite materials (modified para-aramid fibers) after being irradiated with ultraviolet rays for different periods of time, and the strength of the composite materials (modified para-aramid fibers) not irradiated with ultraviolet rays is taken as 100%.
[0121] The test method for the relative viscosity retention rate is as follows: the Ubbelohde viscometer is used to test the specific viscosity of the same group of composite materials (para-aramid fiber after modification) after being irradiated with ultraviolet light for different periods of time, and the specific viscosity of the composite material (para-aramid fiber after modification) not irradiated with ultraviolet light is taken as 100%.
[0122] Table 1 Modulus retention of para-aramid fiber
[0123]
[0124] Table 2 Tensile strength retention of para-aramid fiber
[0125]
[0126] Table 3 Specific viscosity retention of para-aramid fiber
[0127]
[0128] From the comparison of the data of Examples 1 to 5 and the blank example, it can be seen that the para-aramid fibers treated by the preparation method of the present invention in Examples 1 to 5 have good resistance to ultraviolet aging. As the ultraviolet irradiation time increases, the modulus, tensile strength and relative viscosity of the aramid fibers do not decrease significantly, and the aramid fibers can be well used in smart wearables, aerospace, automotive industry, sports equipment and other fields.
[0129] From the comparison of the data of Example 1 and Comparative Examples 1 and 2, it can be seen that when the para-aramid fiber is modified by DAE and PANI together, the UV resistance of the para-aramid fiber can be effectively improved. If DAE (Comparative Example 1) is not added, the modulus, strength and specific viscosity of the para-aramid fiber will decrease significantly with the increase of ultraviolet irradiation time, because the molecular structure of DAE will change after absorbing ultraviolet rays, and this change in molecular structure is reversible. Therefore, DAE can continuously absorb ultraviolet rays, thereby reducing the loss of modulus, strength and specific viscosity of the para-aramid fiber exposed to ultraviolet rays for a long time; if PANI (Comparative Example 2) is not added, the comprehensive UV resistance of the para-aramid fiber will decrease, because after DAE completely absorbs ultraviolet rays, the structure changes from an open-loop state to a closed-loop state, and DAE in a closed-loop state does not have the ability to absorb ultraviolet rays. During this period, PANI is required to absorb ultraviolet rays to reduce the loss of modulus, strength and specific viscosity of the para-aramid fiber. Therefore, the synergistic combination of DAE and PANI is conducive to improving the UV aging resistance of the para-aramid fiber. In addition, in the preparation method of the present invention, DAE and PANI are used to sequentially treat the para-aramid fiber, so that the final para-aramid fiber has better fatigue resistance to ultraviolet aging. The tensile strength retention rate of the para-aramid fiber prepared in Example 1 was measured, and its tensile strength retention rate was 80.6% at 30 days, while the tensile strength retention rates of the para-aramid fibers of Comparative Examples 1 and 2 were 62.7% and 64.3% at 30 days, respectively. It can be seen that the para-aramid fiber with ultraviolet resistance and intelligent color change prepared by the method of the present invention has better fatigue resistance.
[0130] From the comparison of the data of Example 1 and Comparative Example 3, it can be seen that if the processing steps of DAE and PANI are replaced, the UV resistance of the para-aramid fiber will also decrease. This is because if the para-aramid fiber is first treated in a PANI organic solution, the amide bonds of the para-aramid fiber will preferentially form hydrogen bonds with the amino groups of PANI, and then when treated with a DAE organic solution, some of the aldehyde groups of DAE will form hydrogen bonds with PANI instead of with the amide bonds of the para-aramid fiber, resulting in a decrease in the UV resistance of the para-aramid fiber.
[0131] From the comparison of the data of Example 1 and Comparative Example 4, it can be seen that if the concentration of DAE is too high, the performance of the para-aramid fiber will also be affected, because the excess DAE cannot form hydrogen bonds with the amide bonds of the para-aramid fiber, thereby causing the modified para-aramid fiber to become brittle.
[0132] From the comparison of the data of Example 1 and Comparative Examples 5 and 6, it can be seen that if the modification treatment temperature of DAE or PANI is lowered, the UV resistance of the modified para-aramid fiber will be reduced. This is because the mobility between DAE or PANI molecules is reduced, and the chance of the aldehyde group of DAE or the amino group of PANI to form hydrogen bonds with the amide bonds of the para-aramid fiber is reduced, so that the DAE or PANI that has not formed hydrogen bonds with the amide bonds of the para-aramid fiber can be easily removed by washing with distilled water and ethanol.
[0133] In summary, the para-aramid fiber treated by the preparation method of the present invention has good UV aging resistance and higher fatigue resistance. In addition, the para-aramid fiber treated by the preparation method of the present invention has good strength performance. In order to form a comparison of strength performance, the following comparative example 7 is added.
[0134] Comparative Example 7
[0135] Zinc oxide is used to treat para-aramid fiber. The specific preparation process is as follows:
[0136] (1) At 60°C, zinc acetate was dissolved in ethanol to obtain a zinc acetate solution with a concentration of 0.1 mol / L, and then 32 mg of sodium hydroxide was added to 140 mL of ethanol, and then 1 g of polyethylene glycol was added to obtain an alkaline solution, and the zinc acetate solution and the alkaline solution were fully mixed to obtain a clear and transparent ZnO seed solution with a concentration of 0.1 mol / L;
[0137] (2) adding DA to a 10 mM tris(hydroxymethyl)aminomethane solution to obtain a 2 g / L DA solution, adjusting the pH of the DA solution to 8.5 using sodium hydroxide, shaking the para-aramid fiber in the DA solution at room temperature for 24 hours, and drying to obtain pretreated para-aramid fiber;
[0138] (3) The pretreated para-aramid fiber is immersed in a ZnO seed solution, slowly stirred for 30 minutes, and dried to obtain the treated para-aramid fiber.
[0139] The strength performance of the para-aramid fibers treated in the above Example 1, Comparative Examples 1-2 and Comparative Example 7 was tested. The specific results are shown in Table 4 below, where the strength performance test method is: GB / T 14344 Chemical Fiber Filament Tensile Performance Test Method.
[0140] Table 4 Strength performance data
[0141]
[0142] It can be seen from the data in Table 4 above that the para-aramid fiber treated by the preparation method of Example 1 still has good strength performance, because DAE and PANI prepared by the present invention contain oxygen atoms and nitrogen atoms with large electronegativity and small radius, respectively, which can form intermolecular hydrogen bonding forces with the hydrogen atoms on the amide bonds of the para-aramid fiber.
[0143] From the data comparison of Example 1 and Comparative Examples 1-2, it can be seen that when DAE and PANI are used together to treat para-aramid fiber, it is more conducive to making the para-aramid fiber have good strength performance. If DAE or PANI is used alone, the strength performance of the para-aramid fiber will be reduced. Because DAE and PANI prepared by the present invention both contain aromatic rings, partial π-π stacking occurs between DAE, PANI and the aromatic heterocyclic rings of para-aramid fiber.
[0144] From the comparison of the data of Example 1 and Comparative Example 7, it can be seen that the para-aramid fiber treated by the preparation method of the present invention has more advantages than the conventional zinc oxide treatment method in terms of resistance to ultraviolet aging and fatigue performance. At the same time, the preparation method of the present invention is more conducive to making the para-aramid fiber have good strength performance, because zinc oxide as an inorganic compound has poor interaction with para-aramid fiber, and its binding ability is far weaker than DAE and PANI that can form intermolecular forces with para-aramid fiber.
[0145] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0146] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A method for preparing a para-aramid fiber with UV resistance and intelligent color change, characterized in that: The preparation method is: S1. Place clean para-aramid fiber in a diarylethene DAE organic solution for modification to obtain aramid fiber DAE-THFL; the concentration of the DAE organic solution is 300-900 μM; S2, placing the aramid fiber DAE-THFL in a PANI organic solution and controlling the reaction temperature, and after the reaction is completed, washing and drying to obtain the ultraviolet resistant intelligent color-changing para-aramid fiber; The modification treatment conditions of step S1 are carried out under oscillation or ultrasonic conditions, the treatment temperature is 55-65° C., and the treatment time is 20-40 min; In step S2, the reaction process is carried out under oscillation or ultrasonic conditions, the reaction temperature is 55-65° C., and the reaction time is 3-6 hours.
2. The method for preparing a para-aramid fiber with UV resistance and intelligent color change according to claim 1, characterized in that: The DAE organic solution is prepared by dissolving DAE in an organic solvent, and the PANI organic solution is prepared by dissolving PANI in an organic solvent, wherein the organic solvent is N-methylpyrrolidone or N,N-dimethylformamide.
3. The method for preparing a para-aramid fiber with UV resistance and intelligent color change according to claim 1, characterized in that: The DAE is (1-(5-formyl-2-methylthiophene-3-yl), 2-(1-methyl-2-methyl-indol-3-yl)) perfluorocyclopentene.
4. The method for preparing a para-aramid fiber with UV resistance and intelligent color change according to claim 1, characterized in that: The concentration of the PANI organic solution is 0.4-0.6 mg / mL.
5. The method for preparing a para-aramid fiber with UV resistance and intelligent color change according to claim 4, characterized in that: The dosage ratio of the para-aramid fiber, the DAE organic solution and the PANI organic solution is (3-5) g: (40-60) mL: (80-120) mL.
6. The method for preparing a para-aramid fiber with UV resistance and intelligent color change according to claim 1, characterized in that: During the washing, distilled water and ethanol are used in sequence for washing; the drying temperature is 65-75°C.
7. A para-aramid fiber with UV resistance and intelligent color change, characterized in that: The para-aramid fiber with UV resistance and intelligent color change is prepared by the preparation method described in any one of claims 1 to 6.
8. An application of the para-aramid fiber resistant to ultraviolet light and intelligent color change according to claim 7, characterized in that: The para-aramid fiber with UV resistance and intelligent color change is used in the fields of smart wearables, aerospace, automobile industry and sports equipment.