Alcohol modified silica sol hybridized polyacrylate emulsion and preparation method thereof

By combining the alcohol-modified silica sol with acrylate monomer, an alcohol-modified silica sol hybrid polyacrylate emulsion is formed, which solves the problem of insufficient mechanical properties and water resistance of the polyacrylate emulsion, and significantly improves its mechanical properties and Weather resistance, suitable for high-performance water-based coatings.

CN119060241APending Publication Date: 2024-12-03NANJING INST GENERAL INST OF COAL SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411307769.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The lack of mechanical properties, water resistance and weather resistance of polyacrylate emulsions limits its application areas.

Method used

The alcohol-modified silica sol is combined with acrylate monomers, and by adjusting the pH value and temperature, an alcohol-modified silica sol hybrid polyacrylate emulsion is formed to enhance its mechanical properties and water resistance.

Benefits of technology

It significantly improves the density and weather resistance of the adhesive film, with water absorption rate ≤3.5%, and weather resistance ≥540h. It is suitable for water-based wood paints and building paints.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides an alcohol-modified silica sol hybridized polyacrylate emulsion with better water resistance and weather resistance and a preparation method thereof. The alcohol-modified silica sol hybridized polyacrylate emulsion is prepared from the following components in parts by mass: 5 to 20 parts of alcohol-modified silica sol, 40 to 70 parts of deionized water, 40 to 70 parts of acrylate monomer, 0.2 to 0.4 part of initiator, 0.6 to 3 parts of emulsifier and 0.1 to 0.4 part of buffering agent. The preparation method comprises the following steps: mixing acidic silica sol and alcohol, adjusting the pH value to 3-4 by using diluted hydrochloric acid, and stirring at normal temperature to obtain alcohol modified silica sol; the preparation method comprises the following steps: uniformly mixing and stirring part of deionized water, part of an emulsifier and an acrylate monomer to obtain a monomer pre-emulsion; and adding the alcohol-modified silica sol, the rest deionized water, part of the initiator solution, an emulsifier and a buffer agent into a reactor, simultaneously heating to 80-85 DEG C, dropwise adding the monomer pre-emulsion and the rest of the initiator solution, and carrying out heat preservation after polymerization to obtain the alcohol-modified silica sol hybridized polyacrylate emulsion which is used as a water-borne wood coating, a building anticorrosive coating and a waterproof coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyacrylate emulsion polymerization, and particularly relates to an alcohol-modified silica sol hybrid polyacrylate emulsion and a preparation method thereof. Background Art

[0002] Water-based paint is safe and environmentally friendly, and is used to replace solvent-based paints that are highly polluting. Polyacrylate emulsion is a general term for various acrylic monomer copolymers. It has the advantages of good film-forming properties, simple construction, and low cost. It is widely used in various industries, especially in the wood paint industry and the construction industry. However, the mechanical properties, water resistance, and weather resistance of polyacrylate emulsion still need to be improved, and silica sol hybrid polyacrylate emulsion is an important way to improve the performance of emulsions. The modified polyacrylate emulsion has excellent water resistance and mechanical properties, which expands the application field and has a good application prospect. Summary of the invention

[0003] The purpose of the present invention is to provide an alcohol-modified silica sol hybrid polyacrylate emulsion in view of the deficiencies of the prior art, which has good water resistance and stability, and a simple production method and low cost.

[0004] To achieve the above object, the present invention adopts the following technical solution:

[0005] An alcohol-modified silica sol hybrid polyacrylate emulsion, the formula composition of which is as follows by weight: 5-20 parts of alcohol-modified silica sol, 40-70 parts of deionized water, 40-70 parts of acrylate monomers, 0.2-0.4 parts of initiator, 0.6-3 parts of emulsifier, and 0.1-0.4 parts of buffer;

[0006] The alcohol-modified silica sol is obtained by mixing acidic silica sol and alcohol, adjusting the pH to 3-4 with dilute hydrochloric acid, and stirring at room temperature; the amount of alcohol added is 10-30% of the mass of the acidic silica sol; the alcohol is one or more of polyethylene glycol 400, polyethylene glycol 1000, polypropylene glycol 400, polypropylene glycol 600, polypropylene glycol 1000, polypropylene glycol 1500, polyether polyol 204, and polyether polyol 303.

[0007] The above-mentioned alcohol-modified silica sol hybrid polyacrylate emulsion, the acrylic ester monomer is one or more of methyl methacrylate, methyl acrylate, ethyl acrylate, styrene, butyl acrylate, butyl methacrylate, hydroxyethyl acrylate, isooctyl acrylate, isobornyl acrylate, acrylic acid, methacrylic acid.

[0008] In the alcohol-modified silica sol hybrid polyacrylate emulsion, the initiator is one or more of ammonium persulfate, potassium persulfate and sodium persulfate.

[0009] In the alcohol-modified silica sol hybrid polyacrylate emulsion, the buffer is one or more of sodium dihydrogen phosphate, sodium bicarbonate, potassium dihydrogen phosphate, sodium acetate, and potassium bicarbonate.

[0010] The preparation method of the alcohol-modified silica sol hybrid polyacrylate emulsion comprises the following steps:

[0011] (1) Preparation of alcohol-modified silica sol: Acidic silica sol and alcohol are mixed, pH is adjusted to 3-4 with dilute hydrochloric acid, and stirred at room temperature for two hours to obtain modified silica sol;

[0012] (2) preparing a monomer pre-emulsion: mixing and stirring a portion of deionized water, a portion of an emulsifier, and an acrylate monomer to obtain a monomer pre-emulsion;

[0013] (3) preparing an initiator solution: stirring and dissolving an initiator in a portion of deionized water to prepare an initiator solution;

[0014] (4) Add modified silica sol, remaining deionized water, a small amount of initiator solution, emulsifier, and buffer into the reactor, and raise the temperature to 80-85°C at the same time. Slowly drop the monomer pre-emulsion and the remaining initiator solution within 1.5 hours, keep the temperature for 2 hours, cool to 40°C, adjust the pH to weak alkaline, and obtain the alcohol-modified silica sol hybrid polyacrylate emulsion after filtering.

[0015] The preparation method of the alcohol-modified silica sol hybrid polyacrylate emulsion comprises the following steps:

[0016] (1) Preparation of alcohol-modified silica sol: 15 parts of acidic silica sol and 3 parts of polypropylene glycol 1500 were mixed, the pH was adjusted to 3-4 with dilute hydrochloric acid, and stirred at room temperature for two hours to obtain alcohol-modified silica sol;

[0017] (2) preparing a monomer pre-emulsion: 50 parts of deionized water, 1 part of an emulsifier, 25 parts of isobornyl acrylate, 38 parts of isooctyl acrylate, and 2 parts of acrylic acid were stirred uniformly to prepare a monomer pre-emulsion;

[0018] (3) Preparation of initiator solution: Dissolve 0.3 parts of sodium persulfate in deionized water by stirring to prepare an initiator solution.

[0019] (4) Add modified silica sol, 10 parts of deionized water, a small amount of initiator solution, 0.5 parts of emulsifier, and 0.2 parts of sodium acetate into the reactor, stir and heat to 80-85°C, slowly drop the monomer pre-emulsion and the remaining initiator solution within 1.5 hours, keep the reaction warm for 2 hours after the addition is completed, cool to 40°C, adjust the pH to weak alkalinity, and filter to obtain the alcohol-modified silica sol hybrid polyacrylate emulsion.

[0020] The beneficial effects of the present invention are as follows: after using alcohol-modified silica sol, the surface of the silica sol will be covered with a layer of organic carbon chain, which has better bonding with polyacrylate molecules. With the addition of silica sol, after the polyacrylate emulsion forms a film, silicon dioxide fills the gaps in the film, making the film denser and improving the mechanical properties of the film; and silicon dioxide has excellent hydrophobic properties and has a certain shielding effect on water, so the water resistance of the film is significantly improved; silicon dioxide has excellent ultraviolet absorption performance, so the coating has better weather resistance. After testing, the water absorption rate is ≤3.5%, and the weather resistance is ≥540h. The better performance can reach a water absorption rate of ≤2.9% and a weather resistance of ≥620h.

[0021] The water-based resin prepared by the invention has good water resistance, mechanical properties and weather resistance, and can be used as water-based wood coating, waterproof coating and architectural coating. DETAILED DESCRIPTION

[0022] The present invention is further described in detail below in conjunction with specific implementation modes.

[0023] Embodiment 1:

[0024] This embodiment provides a method for preparing an alcohol-modified silica sol hybrid polyacrylate emulsion, comprising the following steps:

[0025] 1. Weigh the following raw materials: 5 parts of acidic silica sol, 1 part of polyethylene glycol 400, 40 parts of deionized water, 20 parts of methyl methacrylate, 20 parts of butyl acrylate, 0.2 parts of potassium persulfate, 0.1 parts of sodium bicarbonate, and 0.6 parts of emulsifier (OP-10: SDS (sodium dodecyl sulfate) mixed in a weight ratio of 1:1).

[0026] 2. Preparation of alcohol-modified silica sol: Add 5 parts of acidic silica sol and 1 part of polyethylene glycol 400 into a stirring kettle, adjust the pH to 3-4 with dilute hydrochloric acid, and stir at room temperature for two hours to obtain alcohol-modified silica sol.

[0027] 3. Add 35 parts of deionized water, 0.5 parts of emulsifier, 20 parts of methyl methacrylate and 20 parts of butyl acrylate into another stirring tank and stir evenly to obtain a monomer pre-emulsion;

[0028] 4. Prepare an initiator solution: Dissolve 0.2 parts of potassium persulfate in deionized water by stirring to prepare an initiator solution;

[0029] 5. Add the alcohol-modified silica sol obtained in step 2, 5 parts of deionized water, a small amount of the initiator solution obtained in step 4, 0.1 parts of emulsifier, and 0.1 parts of sodium bicarbonate into the reactor, stir and heat to 80-85°C, slowly drop the monomer pre-emulsion obtained in step 3 and the remaining initiator solution obtained in step 4 within 1.5 hours, keep the reaction warm for 2 hours after the addition is completed, cool to 40°C, adjust the pH to weak alkalinity, and filter to obtain the alcohol-modified silica sol hybrid polyacrylate emulsion.

[0030] Embodiment 2:

[0031] This embodiment provides a method for preparing an alcohol-modified silica sol hybrid polyacrylate emulsion, comprising the following steps:

[0032] 1. Weigh the following raw materials: 10 parts of acidic silica sol, 2 parts of polyethylene glycol 1000, 40 parts of deionized water, 20 parts of methyl acrylate, 19 parts of butyl acrylate, 1 part of methacrylic acid, 0.2 parts of potassium persulfate, 0.2 parts of sodium bicarbonate, and 0.6 parts of emulsifier (OP-10: SDS (sodium dodecyl sulfate) mixed in a weight ratio of 1:1).

[0033] 2. Preparation of alcohol-modified silica sol: Add 10 parts of acidic silica sol and 2 parts of polyethylene glycol 1000 into a stirring kettle, adjust the pH to 3-4 with dilute hydrochloric acid, and stir at room temperature for two hours.

[0034] 3. In another stirring tank, add 35 parts of deionized water, 0.5 parts of emulsifier, 20 parts of methyl acrylate, 19 parts of butyl acrylate and 1 part of methacrylic acid and stir evenly to prepare a monomer pre-emulsion.

[0035] 4. Prepare an initiator solution: Dissolve 0.2 parts of potassium persulfate in deionized water by stirring to prepare an initiator solution.

[0036] 5. Add modified silica sol, 5 parts of deionized water, a small amount of initiator solution, 0.1 parts of emulsifier, and 0.2 parts of sodium bicarbonate into the reactor, stir and heat to 80-85°C, slowly drop the monomer pre-emulsion and the remaining initiator solution within 1.5 hours, keep warm for 2 hours after the addition is completed, cool to 40°C, adjust the pH to weak alkaline, and filter to obtain the product.

[0037] Embodiment 3:

[0038] This embodiment provides a method for preparing an alcohol-modified silica sol hybrid polyacrylate emulsion, comprising the following steps:

[0039] 1. Weigh the following raw materials: 15 parts of acidic silica sol, 3 parts of polypropylene glycol 1000, 60 parts of deionized water, 25 parts of styrene, 38 parts of isooctyl acrylate, 2 parts of hydroxyethyl acrylate, 0.3 parts of sodium persulfate, 0.2 parts of potassium bicarbonate, and 1.5 parts of emulsifier (OP-10: SDS (sodium dodecyl sulfate) mixed in a weight ratio of 1:1).

[0040] 2. Preparation of alcohol-modified silica sol: Add acidic silica sol and polypropylene glycol 1000 into a stirring kettle, adjust the pH to 3-4 with dilute hydrochloric acid, and stir at room temperature for two hours.

[0041] 3. In another stirring tank, add 50 parts of deionized water, 1 part of emulsifier, styrene, isooctyl acrylate, and hydroxyethyl acrylate and stir evenly to prepare a monomer pre-emulsion.

[0042] 4. Prepare initiator solution: Dissolve sodium persulfate in deionized water by stirring to obtain an initiator solution.

[0043] 5. Add modified silica sol, 10 parts of deionized water, a small amount of initiator solution, 0.5 parts of emulsifier, and potassium bicarbonate into the reactor, stir and heat to 80-85°C, slowly drop the monomer pre-emulsion and the remaining initiator solution within 1.5 hours, keep warm for 2 hours after the addition is complete, cool to 40°C, adjust the pH to weak alkaline, and filter to obtain the product.

[0044] Embodiment 4:

[0045] This embodiment provides a method for preparing an alcohol-modified silica sol hybrid polyacrylate emulsion, comprising the following steps:

[0046] 1. Weigh the following raw materials: 15 parts of acidic silica sol, 3 parts of polypropylene glycol 1500, 60 parts of deionized water, 25 parts of isobornyl acrylate, 38 parts of isooctyl acrylate, 2 parts of acrylic acid, 0.3 parts of sodium persulfate, 0.2 parts of sodium acetate, 1.5 parts of emulsifier (OP-10: SDS (sodium dodecyl sulfate) mixed in a weight ratio of 1:1).

[0047] 2. Preparation of alcohol-modified silica sol: Add acidic silica sol and polypropylene glycol 1500 into a stirring kettle, adjust the pH to 3-4 with dilute hydrochloric acid, and stir at room temperature for two hours.

[0048] 3. In another stirring tank, add 50 parts of deionized water, 1 part of emulsifier, isobornyl acrylate, isooctyl acrylate, and acrylic acid and stir evenly to prepare a monomer pre-emulsion.

[0049] 4. Prepare initiator solution: Dissolve sodium persulfate in deionized water by stirring to obtain an initiator solution.

[0050] 5. Add modified silica sol, 10 parts of deionized water, a small amount of initiator solution, 0.5 parts of emulsifier, and sodium acetate into the reactor, stir and heat to 80-85°C, slowly drop the monomer pre-emulsion and the remaining initiator solution within 1.5 hours, keep warm for 2 hours after the addition is complete, cool to 40°C, adjust the pH to weak alkaline, and filter to obtain the product.

[0051] Embodiment 5:

[0052] This embodiment provides a method for preparing an alcohol-modified silica sol hybrid polyacrylate emulsion, comprising the following steps:

[0053] 1. Weigh the following raw materials: 15 parts of acidic silica sol, 3 parts of polypropylene glycol 600, 60 parts of deionized water, 25 parts of isobornyl acrylate, 38 parts of isooctyl acrylate, 2 parts of acrylic acid, 0.3 parts of sodium persulfate, 0.2 parts of sodium acetate, 1.5 parts of emulsifier (OP-10: SDS (sodium dodecyl sulfate) mixed in a weight ratio of 1:1).

[0054] 2. Preparation of alcohol-modified silica sol: Add acidic silica sol and polypropylene glycol 600 into a stirring kettle, adjust the pH to 3-4 with dilute hydrochloric acid, and stir at room temperature for two hours.

[0055] 3. In another stirring tank, add 50 parts of deionized water, 1 part of emulsifier, isobornyl acrylate, isooctyl acrylate, and acrylic acid and stir evenly to prepare a monomer pre-emulsion.

[0056] 4. Prepare an initiator solution: Dissolve sodium persulfate in deionized water by stirring to prepare an initiator solution.

[0057] 5. Add modified silica sol, 10 parts of deionized water, a small amount of initiator solution, 0.5 parts of emulsifier, and sodium acetate into the reactor, stir and heat to 80-85°C, slowly drop the monomer pre-emulsion and the remaining initiator solution within 1.5 hours, keep warm for 2 hours after the addition is complete, cool to 40°C, adjust the pH to weak alkaline, and filter to obtain the product.

[0058] Embodiment 6:

[0059] This embodiment provides a method for preparing an alcohol-modified silica sol hybrid polyacrylate emulsion, comprising the following steps:

[0060] 1. Weigh the following raw materials: 20 parts of acidic silica sol, 6 parts of polyether polyol 303, 70 parts of deionized water, 15 parts of methyl acrylate, 15 parts of isobornyl acrylate, 38 parts of butyl acrylate, 2 parts of acrylic acid, 0.4 parts of ammonium persulfate, 0.4 parts of sodium acetate, and 3 parts of emulsifier (OP-10: SDS (sodium dodecyl sulfate) mixed in a weight ratio of 1:1).

[0061] 2. Preparation of alcohol-modified silica sol: Add acidic silica sol and polyether polyol 303 into a stirring kettle, adjust the pH to 3-4 with dilute hydrochloric acid, and stir at room temperature for two hours.

[0062] 3. In another stirred tank, add 60 parts of deionized water, 2.5 parts of emulsifier, methyl acrylate, isobornyl acrylate, butyl acrylate and acrylic acid and stir evenly to prepare a monomer pre-emulsion.

[0063] 4. Prepare initiator solution: Dissolve ammonium persulfate in deionized water by stirring to prepare an initiator solution.

[0064] 5. Add modified silica sol, 10 parts of deionized water, a small amount of initiator solution, 0.5 parts of emulsifier, and sodium acetate into the reactor, stir and heat to 80-85°C, slowly drop the monomer pre-emulsion and the remaining initiator solution within 1.5 hours, keep warm for 2 hours after the addition is complete, cool to 40°C, adjust the pH to weak alkaline, and filter to obtain the product.

[0065] The finished products prepared in Examples 1-6 were subjected to various performance tests as shown in the following table, and the results are shown in the following table. The water absorption rate was tested according to the HG / T3344-2012 standard; the weather resistance was tested according to the GB / T 1865-2009 standard artificial aging test.

[0066] Water absorption Weather resistance Example 1 3.2% 600h Example 2 3.1% 580h Example 3 2.9% 540h Example 4 2.9% 620h Example 5 3.5% 630h Example 6 3.3% 600h

[0067] As can be seen from the above table, the present invention has good water resistance and weather resistance, and can be used as water-based wood coatings, waterproof coatings, and building anticorrosive coatings.

Claims

1. An alcohol-modified silica sol hybrid polyacrylate emulsion, characterized in that: The formula composition is as follows by mass: 5-20 parts of alcohol-modified silica sol, 40-70 parts of deionized water, 40-70 parts of acrylate monomers, 0.2-0.4 parts of initiator, 0.6-3 parts of emulsifier, and 0.1-0.4 parts of buffer; The alcohol-modified silica sol is obtained by mixing acidic silica sol and alcohol, adjusting the pH to 3-4 with dilute hydrochloric acid, and stirring at room temperature; the amount of alcohol added is 10-30% of the mass of the acidic silica sol; the alcohol is one or more of polyethylene glycol 400, polyethylene glycol 1000, polypropylene glycol 400, polypropylene glycol 600, polypropylene glycol 1000, polypropylene glycol 1500, polyether polyol 204, and polyether polyol 303.

2. The alcohol-modified silica sol hybrid polyacrylate emulsion according to claim 1, characterized in that: The acrylic acid ester monomer is one or more of methyl methacrylate, methyl acrylate, ethyl acrylate, styrene, butyl acrylate, butyl methacrylate, hydroxyethyl acrylate, isooctyl acrylate, isobornyl acrylate, acrylic acid, and methacrylic acid.

3. The alcohol-modified silica sol hybrid polyacrylate emulsion according to claim 1, characterized in that: The initiator is one or more of ammonium persulfate, potassium persulfate and sodium persulfate.

4. The alcohol-modified silica sol hybrid polyacrylate emulsion according to claim 1, characterized in that: The buffer is one or more of sodium dihydrogen phosphate, sodium bicarbonate, potassium dihydrogen phosphate, sodium acetate and potassium bicarbonate.

5. The method for preparing the alcohol-modified silica sol hybrid polyacrylate emulsion according to claim 1, characterized in that: The following steps are involved: (1) Preparation of alcohol-modified silica sol: Acidic silica sol and alcohol are mixed, pH is adjusted to 3-4 with dilute hydrochloric acid, and stirred at room temperature for two hours to obtain modified silica sol; (2) preparing a monomer pre-emulsion: mixing and stirring a portion of deionized water, a portion of an emulsifier, and an acrylate monomer to obtain a monomer pre-emulsion; (3) preparing an initiator solution: stirring and dissolving an initiator in a portion of deionized water to prepare an initiator solution; (4) Add modified silica sol, remaining deionized water, a small amount of initiator solution, emulsifier, and buffer into the reactor, and raise the temperature to 80-85°C at the same time. Slowly drop the monomer pre-emulsion and the remaining initiator solution within 1.5 hours, keep the temperature for 2 hours, cool to 40°C, adjust the pH to weak alkaline, and obtain the alcohol-modified silica sol hybrid polyacrylate emulsion after filtering.

6. The method for preparing the alcohol-modified silica sol hybrid polyacrylate emulsion according to claim 1, characterized in that: The following steps are involved: (1) Preparation of alcohol-modified silica sol: 15 parts of acidic silica sol and 3 parts of polypropylene glycol 1500 were mixed, the pH was adjusted to 3-4 with dilute hydrochloric acid, and stirred at room temperature for two hours to obtain alcohol-modified silica sol; (2) preparing a monomer pre-emulsion: 50 parts of deionized water, 1 part of an emulsifier, 25 parts of isobornyl acrylate, 38 parts of isooctyl acrylate, and 2 parts of acrylic acid were stirred uniformly to prepare a monomer pre-emulsion; (3) Preparation of initiator solution: Dissolve 0.3 parts of sodium persulfate in deionized water by stirring to prepare an initiator solution. (4) Add modified silica sol, 10 parts of deionized water, a small amount of initiator solution, 0.5 parts of emulsifier, and 0.2 parts of sodium acetate into the reactor, stir and heat to 80-85°C, slowly drop the monomer pre-emulsion and the remaining initiator solution within 1.5 hours, keep the reaction warm for 2 hours after the addition is completed, cool to 40°C, adjust the pH to weak alkalinity, and filter to obtain the alcohol-modified silica sol hybrid polyacrylate emulsion.