A GO-POSS modified wear-resistant antistatic back coating composition and a brightening film

By using graphene oxide-cage silsesquioxane nanoparticles combined with other materials in an optical brightening film, the lack of wear resistance and scratch resistance of the backcoat in the prior art is solved. The risk of antistatic agent precipitation is avoided.

CN117363203BActive Publication Date: 2024-12-03NINGBO EXCITON TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311481354.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-08
Publication Date
2024-12-03
Estimated Expiration
2043-11-08

AI Technical Summary

Technical Problem

The back coated protective layer of the existing optical brightening film is insufficient in cutting and assembly applications, and requires additional antistatic agents to meet resistance requirements, but increases costs and risks of precipitation.

Method used

采用氧化石墨烯-笼型倍半硅氧烷(GO-POSS)作为有机/无机杂化纳米粒子,结合基材连接剂、聚氨酯预聚物和有机微粒,形成一种耐磨抗静电的背涂涂层组合物,通过紫外光固化技术提高附着力和耐刮性。

Benefits of technology

It realizes the adhesion, wear resistance and antistatic properties of the back coating without increasing costs, reduces the white spots and white lines of the diaphragm during the module assembly process, and avoids the precipitation of antistatic agents. risk.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004538341950000121
    Figure BDA0004538341950000121
  • Figure HDA0004538341960000011
    Figure HDA0004538341960000011
  • Figure HDA0004538341960000021
    Figure HDA0004538341960000021
Patent Text Reader

Abstract

A coating composition for a back coating, the coating composition comprising a substrate connector, a polyurethane prepolymer, organic microparticles, and organic / inorganic hybrid nanoparticles, wherein the organic / inorganic hybrid nanoparticles are graphene oxide-cage silsesquioxane (GO-POSS) particles. The back coating composition has excellent wear resistance, scratch resistance, and antistatic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This patent relates to the field of optical film technology, and in particular to a GO-POSS modified wear-resistant and antistatic back coating composition and a brightening film. Background Art

[0002] The optical brightness enhancement films currently used in displays are usually composed of a substrate layer, a prism layer and a back-coating protective layer. However, the wear and scratch resistance of the back-coating protective layer formed by the coating liquid or glue coating provided on the market cannot meet the requirements of many actual cutting and assembly applications, and additional antistatic agents need to be added to meet the back resistance requirements, which increases costs and poses a risk of precipitation.

[0003] CN201010165392.9 discloses a UV-curable hard coating film for improving the scratch resistance, wear resistance and antifouling performance of a plastic film, but its adhesion is only 4B, which is difficult to meet the requirements of an optical film. It also has no antistatic properties and requires the addition of an antistatic agent, which will increase the risk of precipitation after RA.

[0004] CN110079208A discloses a UV-curable composition having high brightness, excellent anti-fouling property and scratch resistance. However, the composition is used for brightening the structural layer and it is uncertain whether it can be used as a back coating protective layer.

[0005] CN101205424A discloses a hard coating composed of ultraviolet light-cured acrylate, thermoplastic resin, photoinitiator, silicone and solvent, characterized in that the coating can inhibit cracking or curling caused by curing shrinkage, and inhibit the adhesion of fingerprints and dust on the surface of the film, but the hardness of the coating is not high enough, and the scratch resistance and wear resistance are limited.

[0006] As an important derivative of graphene materials, graphene oxide (GO) not only maintains the special surface properties and layered structure of graphene, but also has excellent physical, chemical, optical and electrical properties. The oxygen-containing groups on the surface of graphene oxide give it good chemical stability, and the oxygen-containing functional groups are more likely to bond and react chemically with other functional groups.

[0007] Polyhedral oligomeric silsesquioxane (POSS) has a hollow cage structure with Si-O-Si bonds as the inorganic skeleton. Its general formula is generally (RSiO 1.5)n, wherein R represents an organic functional group, such as an inert group such as hydrogen, phenyl, alkyl, or a reactive group such as vinyl, amino, and epoxy, and the inert group can improve the compatibility of POSS with the polymer, while the reactive group can chemically react with the polymer and can be connected to the organic chain in a chemical bonding manner, thereby obtaining an organic-inorganic hybrid nanocomposite material with excellent performance.

[0008] Polyhedral oligomeric silsesquioxane is bonded to modified graphene oxide (GO-POSS) through amide bonds, so that graphene oxide has the good dielectric properties, optical properties, thermal stability, mechanical properties and flame retardancy of polyhedral oligomeric silsesquioxane while taking into account its own excellent properties. It is then grafted onto the polymer molecular chain through the reactive groups on GO-POSS, which significantly improves the heat resistance, flame retardancy, hardness and friction properties of the polymer without affecting the inherent properties of the polymer itself. Summary of the invention

[0009] In view of this, the purpose of this patent is to provide a wear-resistant and antistatic back coating composition and a brightness enhancement film. The back coating composition provided by this patent has excellent wear resistance, scratch resistance and antistatic properties.

[0010] In order to solve the above technical problems, the present patent first provides a coating composition for a back coating layer, wherein the coating composition comprises a substrate connector, a polyurethane prepolymer, organic microparticles, and organic / inorganic hybrid nanoparticles. The organic / inorganic hybrid nanoparticles are graphene oxide-cage silsesquioxane (GO-POSS) particles. The substrate connector comprises acrylate, epoxy acrylate or acrylate copolymer. The substrate connector in the coating composition is 20-50 parts by weight, and the content of the graphene oxide-cage silsesquioxane (GO-POSS) particles is 0.2-10 parts by weight.

[0011] Furthermore, the acrylic copolymer includes one or more of polyurethane acrylate, polyester acrylate, and polyether acrylate.

[0012] The main function of the substrate connector in the coating composition of this patent is to combine with the substrate to improve the adhesion between the coatings.

[0013] Furthermore, the acrylate copolymer is preferably an amino acrylate oligomer containing hydroxyl and carboxyl groups and a PCDL type polyurethane acrylate oligomer.

[0014] Furthermore, the acrylate copolymer is most preferably one of a difunctional aliphatic amino acrylate oligomer, a trifunctional aliphatic amino acrylate oligomer, a difunctional PCDL type polyurethane acrylate oligomer, or a combination of the two.

[0015] Furthermore, the polyurethane prepolymer is a reactive semi-finished product obtained by reacting polyisocyanate and polyol in a certain ratio, and can be purchased on the market, such as Jiangsu Qianmeite Polyurethane New Material Co., Ltd. The main function of the polyurethane prepolymer is to improve the adhesion between the coating and the substrate and the wear resistance of the coating.

[0016] Furthermore, the organic particles are selected from one or a combination of at least two of polymethyl methacrylate particles (PMMA), polybutyl methacrylate particles (PBMA), polyethylene particles (PE), polypropylene particles (PP), polyamide particles (PA), polystyrene particles (PS) or silicone particles. The main function of the organic particles is to increase the roughness of the coating and scatter light.

[0017] Furthermore, the organic microparticles are preferably polymethyl methacrylate particles.

[0018] Further, the structure of the cage-type silsesquioxane of the graphene oxide-cage-type silsesquioxane (GO-POSS) particle is as follows Figure 3 , whose molecular formula is (RSiO 1.5 ) n , R is one or two of active or inactive groups such as acrylate (i.e., acryloyloxypropyl), methacrylate (i.e., methacryloyloxypropyl), vinyl, allyloxy, amino, alkyl, hydroxyl, and aromatic groups, and n is an even number greater than or equal to 8, such as 8, 10, 12, 14, 16, 18, 20, etc.

[0019] Furthermore, the number of R amino groups in the cage-type silsesquioxane is ≥1, for example, 2, 3, 4, 5, 6, 7, or 8.

[0020] Furthermore, the number of vinyl groups R in the cage-type silsesquioxane is ≥1, for example, 2, 3, 4, 5, 6, 7, or 8.

[0021] The main function of the organic / inorganic hybrid nanoparticles is to improve the wear resistance and antistatic properties of the coating.

[0022] Further, the coating composition includes a diluent. Preferably, the diluent is selected from one or a combination of at least two of hydroxyethyl acrylate, trimethylolpropane tri(meth)acrylate (TMPTA), N,N-dimethylacrylamide (NNDMA), tripropylene glycol diacrylate (TPGDA), butyl acrylate, isobornyl acrylate, 1,4-butanediol diacrylate, acrylic acid, 1,6-hexanediol di(meth)acrylate, pentaerythritol tetraacrylate, ethoxylated trimethylolpropane triacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol hexaacrylate (DPHA).

[0023] More preferably, the diluent is most preferably one or a combination of at least two of NNDMA, TPGDA, 1,6-hexanediol di(meth)acrylate, TPPTA, or pentaerythritol tetraacrylate.

[0024] The main function of the diluent is to adjust the viscosity of the composition so as to achieve the purpose of uniform mixing of the feed liquid and suitable coating process.

[0025] Furthermore, the coating composition includes a leveling agent, which may be an organic silicone leveling agent, preferably BYK333, BYK344, etc., whose main component is polyether-modified polydimethylsiloxane.

[0026] The main function of the leveling agent is to increase the leveling property of the coating liquid.

[0027] Furthermore, the coating composition includes a dispersant, which may be a fine dispersant, preferably a polyether surfactant, which may be TEGO688.

[0028] The main function of the dispersant is to improve the dispersibility of the particles in the coating solution.

[0029] Furthermore, the coating composition includes a defoamer, which may be a non-silicon polyether compound, preferably BYK1794.

[0030] The main function of the defoamer is to reduce the generation of bubbles in the coating liquid during use.

[0031] Furthermore, the coating composition includes a photoinitiator, and the photoinitiator is one of BASF's Irgacure 184, Irgacure 754, Irgacure 369, and Irgacure 1173, or a combination of at least two of them.

[0032] More preferably, the photoinitiator is one or a combination of Irgacure 184 and Irgacure 1173.

[0033] Furthermore, the coating composition contains 20-50 parts by weight of the substrate connector, or 25-45 parts by weight, or 30 parts by weight, 35 parts by weight, or 40 parts by weight.

[0034] Furthermore, the polyurethane prepolymer in the coating composition is 20-50 parts by weight, or 25-45 parts by weight, or 30 parts by weight, 35 parts by weight, or 40 parts by weight.

[0035] Furthermore, the organic particles in the coating composition are 0.1-1 parts by weight, or 0.2-0.9 parts by weight, or 0.4 parts by weight, 0.6 parts by weight, or 0.7 parts by weight.

[0036] Furthermore, the coating composition contains 0.5-5 parts by weight, or 0.8-4.5 parts by weight, or 1.5 parts by weight, 2.0 parts by weight, 2.5 parts by weight, 3.0 parts by weight, 3.5 parts by weight, or 4.0 parts by weight of organic / inorganic hybrid nanoparticles.

[0037] Furthermore, the diluent in the coating composition is 20-30 parts by weight, or 23-28 parts by weight, or 25 parts by weight, 26 parts by weight, or 27 parts by weight.

[0038] Furthermore, the coating composition contains 0.1-1 parts by weight, or 0.2-0.9 parts by weight, or 0.3 parts by weight, 0.5 parts by weight, or 0.7 parts by weight of the leveling agent.

[0039] Furthermore, the coating composition contains 1-5 parts by weight of the dispersant, or 1.2-4.5 parts by weight, or 1.5 parts by weight, 2.0 parts by weight, 2.5 parts by weight, 3.0 parts by weight, 3.5 parts by weight, or 4.0 parts by weight.

[0040] Furthermore, the defoaming agent in the coating composition is 0.5-2 parts by weight, or 0.6-1.9 parts by weight, or 0.8 parts by weight, 1.0 parts by weight, 1.5 parts by weight, 1.6 parts by weight, or 1.8 parts by weight.

[0041] Furthermore, the photoinitiator in the coating composition is 1-5 parts by weight, or 1.3-4.5 parts by weight, or 1.5 parts by weight, 2.0 parts by weight, 2.5 parts by weight, 3.0 parts by weight, 3.5 parts by weight, or 4.0 parts by weight.

[0042] The coating composition of this patent is mainly used for the back coating of the brightness enhancement film to improve the wear resistance, scratch resistance and antistatic properties of the back coating surface of the brightness enhancement film.

[0043] This patent also provides a method for preparing a coating composition, including:

[0044] Step (1), adding the raw materials into the barrel according to the raw material ratio;

[0045] Step (2), stirring and ultrasonically dispersing;

[0046] Step (3), filtering to obtain a coating composition.

[0047] This patent also provides a brightness enhancement film, including a brightness enhancement structural layer, a substrate layer and a back coating layer, wherein the back coating layer is prepared by curing the coating composition.

[0048] This patent also provides a method for preparing a brightness enhancement film, comprising a brightness enhancement structure layer, a substrate layer and a back coating layer, wherein the back coating layer is prepared by curing the coating composition, comprising:

[0049] Step (1), coating the coating composition on the lower surface of the substrate layer and curing to obtain a back coating layer;

[0050] Step (2), coating UV glue on the upper surface of the substrate layer, rolling and curing to obtain a brightening structure layer, thereby preparing a brightening film.

[0051] Furthermore, in step (1), the coating composition is uniformly mixed and then coated on the lower surface of the substrate layer, and then dried and cured to obtain a back coating layer.

[0052] Furthermore, in step (1), curing is performed by ultraviolet light irradiation curing.

[0053] Furthermore, in step (2), rolling is performed using a copper roller having a microstructure.

[0054] Furthermore, in step (2), curing is performed by ultraviolet light irradiation curing.

[0055] Furthermore, the curing energy of step (1) and step (2) is 100-500 mj / cm, or 150-450 mj / cm, 200 mj / cm, 250 mj / cm, 300 mj / cm, 350 mj / cm.

[0056] Furthermore, the substrate layer is made of a polymer resin. Preferably, the polymer resin is selected from one or a combination of at least two of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate (PC), polymethyl methacrylate (PMMA), polylactic acid (PLA), or polyester polyurethane (PU).

[0057] Furthermore, the substrate layer is made of a transparent material and has a thickness of 50 μm-300 μm, or 80 μm, 100 μm, 130 μm, 150 μm, 180 μm, 200 μm, 250 μm, or 280 μm.

[0058] Furthermore, the back coating layer is prepared by micro-dimpled coating.

[0059] Furthermore, the thickness of the back coating layer is 2 μm-15 μm, or 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, or 14 μm.

[0060] Furthermore, the brightness enhancement structure layer is a micro-prismatic structure, and the height of the micro-prismatic structure is 10 μm-30 μm, or 13 μm, 15 μm, 18 μm, 20 μm, 25 μm, or 28 μm.

[0061] Furthermore, the brightness enhancement structure layer is a micro-prismatic structure with an edge angle of 85°-95°, or 90°.

[0062] Compared with the prior art, the product provided by this patent has the following advantages or functions:

[0063] The coating composition provided by this patent can have a 5B adhesion on the back coating formed by corona or chemical substrate UV curing, and has better wear resistance, scratch resistance and antistatic properties without affecting the performance, thereby reducing white spots, white lines and other defects of the diaphragm during the module assembly and transportation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 A schematic diagram of the cross-sectional structure of the brightness enhancement film provided by this patent;

[0065] Figure 2 Schematic diagram of the structure of GO-POSS nanoparticles;

[0066] Figure 3 It is a cage-type silsesquioxane structure. DETAILED DESCRIPTION

[0067] In order to make it easier to understand the structure of this patent and the functional features and advantages that can be achieved, the following is a detailed description of the preferred embodiments of this patent with the help of the drawings as follows:

[0068] The GO-POSS particles in the technical solution of the present invention can be prepared by the following method: POSS and GO in a ratio of 1:1 by weight are added to 20 parts by weight of ethyl acetate as a dispersion medium, and dispersed for 1 hour using an ultrasonic disperser, the POSS dispersion is slowly added to the GO dispersion, and 10 parts by weight of phosphorus pentoxide (P 2 O 5 ), and then placed at 60 ° C for 8 h of stirring reaction. After the reaction, the supernatant was poured out by centrifuge, and repeatedly washed with deionized water to obtain GO-POSS nanoparticles.

[0069] The GO-POSS particles in this patented technical solution can also be prepared by other methods.

[0070] The preparation method of the coating composition provided by this patent is: adding the raw materials of the coating composition into a barrel according to a ratio, stirring and ultrasonically dispersing until the mixture is uniform, and filtering to obtain a coating composition that can be coated on a substrate.

[0071] The viscosity of the coating composition was further measured using a Tu-4 cup.

[0072] The method for applying the coating composition provided by this patent to the base coating of a brightening film or a composite film is to use a micro-concave anilox roller to evenly coat the mixed coating composition on the substrate, and then UV cure it under a UV curing lamp.

[0073] like Figure 1 As shown, the brightness enhancement film provided by this patent includes a front structural layer 104, a bonding layer 103, a substrate layer 102, and a back protective layer 101.

[0074] The UV-curable coating composition provided by this patent and the coating formed after curing on the polymer substrate are tested for performance according to the following method:

[0075] Adhesion test: The haze is tested using GB-T9286 standard.

[0076] Hardness test: Use GB-T6739 standard to test haze.

[0077] Wear test: Tested with the national standard method of 0000# steel wool ball. Fix the sample to be tested on the wear machine with the test surface facing up, cut the steel wool into the size of the abrasive tool and glue it to the friction head, and fix it in the fixture; select the appropriate weight and add it to the weight fixing rod above the friction head, gently lower the friction head, contact it with the test surface, and start the test. The moving speed is 8cm / sec, and the number of frictions is ten times back and forth. 15 seconds after the end of the friction, place the film under the lighted desk lamp for reflection observation, the observation distance is 20cm, and observe at a 45-degree angle to the left and right to see if there is obvious abrasion on the film surface; if the coating is not worn under the corresponding gram weight, it is judged to be OK, otherwise continue to increase the gram weight until the abrasion NG appears, and the highest gram weight without abrasion is the wear-resistant weight.

[0078] Scratch resistance test: Refer to the scratch test method of GB / T9279-1988, wipe the coating surface with 0000# steel wool, no scratch is excellent, slight scratch is good, severe scratch is poor.

[0079] RA precipitation test: Place in a damp heat aging box for 200 hours, where the temperature is 65℃±1℃ and the relative humidity is 95%±2%, and then observe the coating surface with a microscope.

[0080] Surface resistance test: The surface resistance value (Ω / □) was measured using a SIMCOST-4 surface resistance value tester.

[0081] The test results are shown in Table 1.

[0082] Example 1

[0083] 25 parts by weight of hydroxyl-containing polyurethane acrylate oligomer, 24 parts by weight of PCDL type polyurethane prepolymer, 0.5 parts by weight of organic particles, 1 part by weight of nano GO-POSS particles, 20 parts by weight of diluent, 0.5 parts by weight of leveling agent, 2.5 parts by weight of dispersant, 0.5 parts by weight of defoamer, and 5 parts by weight of photoinitiator. The organic particles are polymethyl methacrylate particles with a particle size distribution of 1-30 μm, the diluent is N, N-dimethylacrylamide, the leveling agent is BYK333, the defoamer is BYK1794, the dispersant is TEGO688, and the photoinitiator is Irgacure184.

[0084] The coating composition is mixed evenly in proportion, and then the mixed coating composition is evenly coated on a common substrate by a micro-concave anilox roller coating method, baked at 100°C for 1-2 minutes, and then the coating is UV cured with a curing energy of 300mj / c, so that a coating with high adhesion and high scratch resistance can be obtained, and the coating thickness is 2-8μm.

[0085] Example 2

[0086] 25 parts by weight of acrylate copolymer, 24 parts by weight of PCDL type polyurethane prepolymer, 0.5 parts by weight of organic particles, 3 parts by weight of nano GO-POSS particles, 18 parts by weight of diluent, 0.5 parts by weight of leveling agent, 2.5 parts by weight of dispersant, 0.5 parts by weight of defoamer, and 5 parts by weight of photoinitiator. The organic particles are polymethyl methacrylate particles with a particle size distribution of 1-30 μm, the diluent is N, N-dimethylacrylamide, the leveling agent is BYK333, the defoamer is BYK1794, the dispersant is TEGO688, and the photoinitiator is Irgacure184.

[0087] The coating composition is mixed evenly in proportion, and then the mixed coating composition is evenly coated on a common substrate by a micro-concave anilox roller coating method, baked at 100°C for 1-2 minutes, and then the coating is UV cured with a curing energy of 300mj / c, so that a coating with high adhesion and high scratch resistance can be obtained, and the coating thickness is 2-8μm.

[0088] Example 3

[0089] 25 parts by weight of acrylate copolymer, 20 parts by weight of PCDL type polyurethane prepolymer, 0.5 parts by weight of organic particles, 5 parts by weight of nano GO-POSS particles, 20 parts by weight of diluent, 0.5 parts by weight of leveling agent, 2.5 parts by weight of dispersant, 0.5 parts by weight of defoamer, and 5 parts by weight of photoinitiator. The organic particles are polymethyl methacrylate particles with a particle size distribution of 1-30 μm, the diluent is N, N-dimethylacrylamide, the leveling agent is BYK333, the defoamer is BYK1794, the dispersant is TEGO688, and the photoinitiator is Irgacure184.

[0090] The coating composition is mixed evenly in proportion, and then the mixed coating composition is evenly coated on a common substrate by a micro-concave anilox roller coating method, baked at 100°C for 1-2 minutes, and then the coating is UV cured with a curing energy of 300mj / c, so that a coating with high adhesion and high scratch resistance can be obtained, and the coating thickness is 2-8μm.

[0091] Example 4

[0092] 45 parts by weight of PCDL type polyurethane prepolymer, 0.5 parts by weight of organic particles, 5 parts by weight of nano GO-POSS particles, 20 parts by weight of diluent, 0.5 parts by weight of leveling agent, 2.5 parts by weight of dispersant, 0.5 parts by weight of defoamer, and 5 parts by weight of photoinitiator. The organic particles are polymethyl methacrylate particles with a particle size distribution of 1-30 μm, the diluent is N, N-dimethylacrylamide, the leveling agent is BYK333, the defoamer is BYK1794, the dispersant is TEGO688, and the photoinitiator is Irgacure184.

[0093] The coating composition is mixed evenly in proportion, and then the mixed coating composition is evenly coated on a common substrate by a micro-concave anilox roller coating method, baked at 100°C for 1-2 minutes, and then the coating is UV cured with a curing energy of 300mj / c, so that a coating with high adhesion and high scratch resistance can be obtained, and the coating thickness is 2-8μm.

[0094] Example 5

[0095] 45 parts by weight of acrylate copolymer, 0.5 parts by weight of organic particles, 5 parts by weight of nano GO-POSS particles, 20 parts by weight of diluent, 0.5 parts by weight of leveling agent, 2.5 parts by weight of dispersant, 0.5 parts by weight of defoamer, and 5 parts by weight of photoinitiator. The organic particles are polymethyl methacrylate particles with a particle size distribution of 1-30 μm, the diluent is N,N-dimethylacrylamide, the leveling agent is BYK333, the defoamer is BYK1794, the dispersant is TEGO688, and the photoinitiator is Irgacure184.

[0096] The coating composition is mixed evenly in proportion, and then the mixed coating composition is evenly coated on a common substrate by a micro-concave anilox roller coating method, baked at 100°C for 1-2 minutes, and then the coating is UV cured with a curing energy of 300mj / c, so that a coating with high adhesion and high scratch resistance can be obtained, and the coating thickness is 2-8μm.

[0097] Comparative Example 1

[0098] Compared with Example 1, the nano GO-POSS particles are replaced with PCDL type polyurethane prepolymer.

[0099] 25 parts by weight of hydroxyl-containing polyurethane acrylate oligomer, 25 parts by weight of PCDL type polyurethane prepolymer, 0.5 parts by weight of organic particles, 20 parts by weight of diluent, 0.5 parts by weight of leveling agent, 2.5 parts by weight of dispersant, 0.5 parts by weight of defoamer, and 5 parts by weight of photoinitiator. The organic particles are polymethyl methacrylate particles with a particle size distribution of 1-30 μm, the diluent is N,N-dimethylacrylamide, the leveling agent is BYK333, the defoamer is BYK1794, the dispersant is TEGO688, and the photoinitiator is Irgacure184.

[0100] The coating composition is mixed evenly in proportion, and then the mixed coating composition is evenly coated on a common substrate by a micro-concave anilox roller coating method, baked at 100°C for 1-2 minutes, and then the coating is UV cured with a curing energy of 300mj / c to obtain a coating with a coating thickness of 2 to 8μm.

[0101] Comparative Example 2

[0102] 50 parts by weight of PCDL type polyurethane prepolymer, 0.5 parts by weight of organic particles, 20 parts by weight of diluent, 0.5 parts by weight of leveling agent, 2.5 parts by weight of dispersant, 0.5 parts by weight of defoamer, and 5 parts by weight of photoinitiator. The organic particles are polymethyl methacrylate particles with a particle size distribution of 1-30 μm, the diluent is N, N-dimethylacrylamide, the leveling agent is BYK333, the defoamer is BYK1794, the dispersant is TEGO688, and the photoinitiator is Irgacure184. The coating composition is mixed evenly according to the proportion, and then the mixed coating composition is evenly coated on a common substrate by a micro-concave anilox roller coating method, baked at 100°C for 1-2 minutes, and then the coating is UV cured with a curing energy of 300 mj / c to obtain a coating with a coating thickness of 2 to 8 μm.

[0103] Comparative Example 3

[0104] 50 parts by weight of acrylate copolymer, 0.5 parts by weight of organic particles, 20 parts by weight of diluent, 0.5 parts by weight of leveling agent, 2.5 parts by weight of dispersant, 0.5 parts by weight of defoamer, and 5 parts by weight of photoinitiator. The organic particles are polymethyl methacrylate particles with a particle size distribution of 1-30 μm, the diluent is N,N-dimethylacrylamide, the leveling agent is BYK333, the defoamer is BYK1794, the dispersant is TEGO688, and the photoinitiator is Irgacure184.

[0105] The coating composition is mixed evenly in proportion, and then the mixed coating composition is evenly coated on a common substrate by a micro-concave anilox roller coating method, baked at 100°C for 1-2 minutes, and then the coating is UV cured with a curing energy of 300mj / c to obtain a coating with a coating thickness of 2 to 8μm.

[0106] Table 1 Example

[0107]

[0108] Note: Maximum weight is 2000g

[0109] It can be concluded from the test results of the above embodiments and comparative examples that the coating composition provided by this patent can improve the wear resistance, scratch resistance and antistatic properties of the coating by adjusting the proportion of GO-POSS nanoparticles while ensuring 5B adhesion to the substrate, and there is no precipitation after RA.

[0110] The above is only a preferred embodiment of this patent and is not intended to limit the scope of protection of this patent. All equivalent changes and modifications made based on the content of this patent are included in the patent scope of this patent.

Claims

1. A method for preparing a back coating composition, the coating composition comprising a substrate linker, a polyurethane prepolymer, organic microparticles, and organic / inorganic hybrid nanoparticles; The substrate connector includes epoxy acrylate or acrylate copolymer; The polyurethane prepolymer is a reactive semi-finished product obtained by reacting polyisocyanate and polyol in a certain ratio; The organic particles are selected from one or a combination of at least two of polymethyl methacrylate particles, polybutyl methacrylate particles, polyethylene particles, polypropylene particles, polyamide particles or silicone particles; The organic / inorganic hybrid nanoparticles are graphene oxide-cage silsesquioxane (GO-POSS) particles, and the molecular formula of the cage silsesquioxane of the graphene oxide-cage silsesquioxane (GO-POSS) particles is (RSiO 1.5 ) n , n is an even number greater than or equal to 8, and R is one or two active or inactive groups selected from acrylate, methacrylate, vinyl, allyloxy, amino, alkyl, hydroxyl, and aryl groups; The coating composition contains 20-50 parts by weight of a substrate connector, 20-50 parts by weight of a polyurethane prepolymer, 0.1-1 parts by weight of organic particles, and 0.2-10 parts by weight of graphene oxide-cage silsesquioxane (GO-POSS) particles. in, Step (1), adding the coating composition into a barrel according to the raw material ratio; Step (2), stirring and ultrasonically dispersing; Step (3), filtering to obtain a coating composition.

2. The method for preparing the coating composition according to claim 1, characterized in that: The acrylate copolymer includes one or more of polyurethane acrylate, polyester acrylate, and polyether acrylate.

3. The method for preparing the coating composition according to claim 1, characterized in that: The preparation method of the graphene oxide-cage silsesquioxane (GO-POSS) particles comprises: adding 1:1 weight parts of POSS and GO to 20 weight parts of dispersion medium ethyl acetate respectively, dispersing for 1 hour using an ultrasonic disperser, slowly adding the POSS dispersion into the GO dispersion, and gradually adding 10 weight parts of phosphorus pentoxide, and then placing at 60° C. for stirring reaction for 8 hours, centrifuging and pouring out the supernatant after the reaction is completed, and repeatedly washing with deionized water to obtain GO-POSS nanoparticles.

4. The method for preparing the coating composition according to claim 1 or 2, characterized in that: n is one of 8, 10, 12, 14, 16, 18 and 20.

5. A brightness enhancement film comprising a brightness enhancement structural layer, a substrate layer and a back coating layer, wherein the back coating layer is prepared by curing a coating composition obtained by the method for preparing a coating composition according to any one of claims 1 to 4.

6. A method for preparing a brightness enhancement film, comprising a brightness enhancement structure layer, a substrate layer and a back coating layer, wherein the back coating layer is prepared by curing a coating composition obtained by the method for preparing a coating composition according to any one of claims 1 to 4, comprising: Step (1), coating the coating composition on the lower surface of the substrate layer by a micro-concave anilox roller coating method, and obtaining a back coating layer after baking and UV curing, wherein the back coating layer has a thickness of 2 to 8 μm, an adhesion of 5B, a hardness of 5H, and a wear resistance of greater than 2000 g; Step (2), coating UV glue on the upper surface of the substrate layer, rolling and curing to obtain a brightening structure layer, thereby preparing a brightening film.

7. The preparation method according to claim 6, characterized in that: Step (1), the coating composition is uniformly mixed and then coated on the lower surface of the substrate layer, and then dried and solidified to obtain a back coating layer.

8. The preparation method according to claim 6, characterized in that: Step (2), rolling using a copper roller having a microstructure.

9. The preparation method according to claim 6, characterized in that: The curing energy of step (1) and step (2) is 100-500 mj / cm.

Citation Information

Patent Citations

  • Hard paint film

    CN101205424A

  • Ultraviolet-cured hard coating and application thereof

    CN102236113A

  • Basal membrane of composite brightness enhancement film

    CN105353431A

  • Composition, BEF (brightness enhancement film) and application of BEF