A dispensing process and its application in fuel cell membrane electrode assemblies
By using diluted water-based pressure-sensitive adhesive and thickener, and designing a mask structure, the problem of uneven adhesive layer thickness and contour in the fuel cell membrane electrode dispensing process was solved, achieving uniformity and stability of ultra-thin adhesive lines, and improving the performance and safety of fuel cells.
Patent Information
- Application Number
- CN202311346423.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-10-18
AI Technical Summary
The existing dispensing process for fuel cell membrane electrodes results in excessively thick adhesive layers and uneven adhesive line contours, which affects fuel cell performance and poses safety hazards. At the same time, the adhesive is prone to overflow and block the gas flow channels.
A water-based pressure-sensitive adhesive latex is diluted with a low-boiling-point alcohol solvent, a thickener is added to adjust the viscosity, and an external mask structure is added to the spray valve of the dispensing machine to control the width and contour of the adhesive line. The support material is then treated with plasma to improve the bonding performance.
It achieves an ultra-thin adhesive line thickness of less than 15μm, improves the uniformity of the adhesive line contour, avoids adhesive layer overflow, and enhances the bonding strength and performance stability of fuel cells.
Smart Images

Figure CN117380501B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a dispensing process and its application in fuel cell membrane electrodes. Background Art
[0002] Proton exchange membrane fuel cells (PEMFC) are composed of multiple single cells connected in series, and each single cell is mainly composed of a membrane electrode (MEA) and a bipolar plate. MEA is the core component of PEMFC and is a key factor affecting PEMFC specific power density, energy density distribution and working life. MEA is mainly composed of a catalyst layer (CL), a proton exchange membrane (PEM) and a gas diffusion layer (GDL). The mainstream MEA preparation method is to coat or thermally transfer the catalyst on both sides of the PEM to obtain a catalyst-coated proton membrane (CCM), and then bond the CCM to the support material with an adhesive to obtain a five-in-one sample, and then bond the GDL to the support material with an adhesive to obtain a seven-layer MEA.
[0003] For the bonding of GDL and five-in-one samples, since thermosetting glue requires high temperature curing, it is easy to cause warping and deformation of GDL and supporting materials. Light-curing glue needs to be dispensed on the black opaque porous GDL, resulting in the risk that the light-curing glue that penetrates into the GDL cannot be completely cured. Therefore, the GDL dispensing glue needs to meet the requirements of having initial adhesion and being able to bond GDL and supporting materials well at low temperatures. Water-based pressure-sensitive glue is currently the most commonly used GDL glue.
[0004] In the structure of existing membrane electrode products, GDL is usually fixed by dispensing glue onto carbon paper along a certain path and width. The thickness is generally more than 30 microns, and there are problems such as uneven glue line contour and difficult to control glue width. The overall thickness of the membrane electrode is often determined by the thickness of the overlapping area of the dispensing glue. The membrane electrode produced by the current dispensing glue process often has destructive cracks and other defects due to the excessive thickness of the glue layer under the tightening pressure of the stack assembly, which leads to "overpressure" at the corresponding position on the bipolar plate, thus affecting the overall performance of the fuel cell and even bringing safety hazards of reaction gas leakage. On the other hand, under the high pressure and high humidity environment of the stack, the glue will also overflow into the gas flow channel of the bipolar plate, blocking the gas flow channel and causing resistance to the flow of gas, thereby affecting the performance of the fuel cell. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a dispensing process and its application in fuel cell membrane electrodes. The present invention can significantly reduce the thickness of the dispensing glue layer, improve the glue line profile and glue width uniformity, and achieve effective bonding of the gas diffusion layer and prevent GDL glue from overflowing.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] In a first aspect, the present invention provides a dispensing process, comprising the following steps:
[0008] (1) diluting an aqueous pressure-sensitive adhesive emulsion with a mixed solvent of water and alcohol to obtain a mixed solution, wherein the solid content of the pressure-sensitive adhesive in the mixed solution is 5-40%;
[0009] (2) adding a thickener to the mixed solution and mixing them uniformly to obtain a dispensing solution, wherein the mass ratio of water to the alcohol solvent in the dispensing solution is (9-5): (1-5), and the viscosity of the dispensing solution is 50-200 cp;
[0010] (3) dispensing the dispensing solution obtained in step (2) on the surface of the gas diffusion layer using a dispensing machine, wherein an external split mask structure is provided below the spray valve on the dispensing machine, the mask structure is connected to the outside of the spray valve needle through a thread or a buckle, and the mask structure is also provided with a built-in slit;
[0011] (4) Pressing the gas diffusion layer obtained in step (3) onto the membrane electrode support material.
[0012] The present invention dilutes the water-based pressure-sensitive adhesive emulsion by using a low-boiling point alcohol solvent and water, so that the solid content of the commercially available water-based pressure-sensitive adhesive emulsion is reduced from 60-70% to 5-40%, and the thickness of the glue line after drying can be effectively made less than 15 μm, thus realizing an ultra-thin glue line. If the solid content of the pressure-sensitive adhesive in the mixed liquid is too high or too low, the thickness of the glue line will be affected.
[0013] At the same time, the mass ratio of water and alcohol solvent in the final glue dispensing solution is controlled, the polarity of the alcohol solvent is regulated, and the partial penetration of the glue dispensing solution in the porous layer on the surface of the super-hydrophobic GDL is promoted, so that the glue line can more effectively "grasp" the gas diffusion layer. If the content of the alcohol solvent is too low, the rapid partial penetration of the glue dispensing solution on the surface of the GDL cannot be achieved. If the content of the alcohol solvent is too high, it will cause the glue dispensing solution to over-penetrate or completely penetrate into the GDL before drying, resulting in too little residual glue on the surface of the GDL, affecting the bonding performance. In addition, the present invention adds a thickener to the glue dispensing solution to increase the viscosity of the glue dispensing solution to 50-200cp. The increase in the viscosity of the glue dispensing solution can effectively prevent the diffusion of the glue line in the plane direction of the GDL surface, making the glue line contour uniform.
[0014] On the other hand, the present invention further controls the dispensing solution and the glue line width and contour edge by adding an external split mask structure to the dispensing machine spray valve. The mask structure is connected to the outside of the dispensing valve needle through a thread or a buckle, and the slit width of the mask structure is adjusted to further control the glue line width and improve the uniformity of the glue line contour.
[0015] Preferably, the alcohol solvent in step (1) is at least one of ethanol, propanol, butanol, ethylene glycol, ethoxyethanol and methoxyethanol.
[0016] Preferably, in step (1), the mass ratio of the aqueous pressure-sensitive adhesive latex, water and alcohol is 1:(0.1-10):(0.1-5).
[0017] Preferably, the mass ratio of water to alcohol solvent in the dispensing solution in step (2) is 8:2.
[0018] Preferably, the thickener in step (2) is an organic compound that does not contain nitrogen.
[0019] The present invention adopts a thickener that does not contain nitrogen, which can avoid the influence of nitrogen on the fuel cell.
[0020] More preferably, the thickener in step (2) is at least one of carbomer resin, polyacrylic acid, and cellulose ether.
[0021] Preferably, the mass of the thickener in step (2) is 0.1-0.5% of the mass of the mixed solution.
[0022] The present invention can effectively prevent the glue line from spreading on the GDL surface by controlling the content of the thickener, which is beneficial to further improve the uniformity of the glue line profile.
[0023] Preferably, in step (3), the distance between the mask structure and the gas diffusion layer is 0.05-3 mm.
[0024] In the dispensing process of the present invention, the mask structure does not directly contact the gas diffusion layer, and the height is adjusted to keep the distance from the gas diffusion layer less than 3 mm, thereby preventing the mask from damaging the surface of the gas diffusion layer and effectively controlling the glue line width.
[0025] Preferably, in step (3), the contact angle of the dispensing solution on the surface of the gas diffusion layer is 60°-130°.
[0026] The present invention can effectively improve the bonding performance between the dispensing solution and the gas diffusion layer by controlling the contact angle within the above range, and avoid excessive penetration or overflow of the dispensing solution on the surface of the gas diffusion layer during dispensing.
[0027] Preferably, the slit width of the mask structure in step (3) is 0.5-5 mm.
[0028] Preferably, in step (4), the membrane electrode support material is pre-treated with plasma.
[0029] The present invention treats the inactive area of the supporting material of the five-in-one MEA through plasma, thereby improving the surface bonding property of the supporting material and further enhancing the bonding force between the ultra-thin glue line and the five-in-one MEA.
[0030] Preferably, in step (4), the pressure when the gas diffusion layer and the membrane electrode support material are pressed is 0.05-0.3 MPa, and the pressing time is 5-30 s.
[0031] The present invention controls the pressure during pressing within the above range, which is beneficial to improving the bonding performance between the gas diffusion layer and the five-in-one MEA and effectively avoiding the destruction of the porous structure of the gas diffusion layer.
[0032] In a second aspect, the present invention also provides an application of a dispensing process in a fuel cell membrane electrode.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The present invention dilutes the aqueous pressure-sensitive adhesive emulsion through a mixed solution of a low-polarity, low-boiling-point alcohol solvent and water, thereby reducing the solid content of the commercially available aqueous pressure-sensitive adhesive from 60-70% to 5-40%, which can effectively make the thickness of the glue line less than 15 μm after drying, thereby achieving an ultra-thin glue line. At the same time, the mass ratio of water and alcohol solvent in the final glue solution is controlled, the polarity of the alcohol solvent is regulated, and the partial penetration of the glue solution in the porous layer on the surface of the super-hydrophobic GDL is promoted, so that the glue line can more effectively "grasp" the gas diffusion layer. In addition, the present invention adds a thickener to the glue solution to increase the viscosity of the glue solution. The increase in the viscosity of the glue solution can effectively prevent the diffusion of the glue line in the plane direction of the GDL surface, making the glue line contour uniform.
[0035] (2) The present invention further controls the dispensing solution and the glue line width and contour edge by adding an external split mask structure to the dispensing machine spray valve. The mask structure is connected to the outside of the dispensing valve needle through a thread or a buckle, and the slit width of the mask structure is adjusted to further control the glue line width and improve the uniformity of the glue line contour. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a structural schematic diagram of the spray valve of the glue dispensing machine in the present invention.
[0037] Figure 2 Schematic diagram of the mask structure in the present invention.
[0038] Figure 3 It is a schematic diagram of the pressure distribution of the adhesive line bonding area under pressure in Example 1 of the present invention.
[0039] Figure 4 It is a schematic diagram of the pressure distribution of the adhesive line bonding area under pressure in Example 2 of the present invention.
[0040] Figure 5 It is a schematic diagram of the pressure distribution of the glue line bonding area under pressure in Example 3 of the present invention.
[0041] Figure 6 It is a schematic diagram of the pressure distribution of the glue line bonding area under pressure in Comparative Example 1 of the present invention.
[0042] Figure 7 It is a schematic diagram of the pressure distribution of the adhesive line bonding area under pressure in Comparative Example 2 of the present invention.
[0043] Figure 8 It is a schematic diagram of the pressure distribution of the glue line bonding area under pressure in Comparative Example 3 of the present invention.
[0044] Fig. 9 It is a schematic diagram of the pressure distribution of the glue line bonding area under pressure in Comparative Example 4 of the present invention.
[0045] Fig.10 It is a schematic diagram of the pressure distribution of the glue line bonding area under pressure in Comparative Example 5 of the present invention.
[0046] Fig.11 It is a schematic diagram of the pressure distribution of the glue line bonding area under pressure in Comparative Example 6 of the present invention.
[0047] Fig.12 It is a schematic diagram of the glue line in Example 1 of the present invention under a microscope.
[0048] Fig.13 It is a schematic diagram of the glue line in Example 2 of the present invention under a microscope.
[0049] Fig.14 It is a schematic diagram of the glue line in Example 3 of the present invention under a microscope.
[0050] Fig.15 It is a schematic diagram of the glue line in Comparative Example 1 of the present invention under a microscope.
[0051] Fig.16 It is a schematic diagram of the glue line in Comparative Example 2 of the present invention under a microscope.
[0052] Fig.17 It is a schematic diagram of the glue line in Comparative Example 3 of the present invention under a microscope.
[0053] Fig.18 It is a schematic diagram of the glue line in Comparative Example 4 of the present invention under a microscope.
[0054] Fig.19 It is a schematic diagram of the glue line in Comparative Example 5 of the present invention under a microscope.
[0055] Fig. 20 It is a schematic diagram of the glue line in Comparative Example 6 of the present invention under a microscope.
[0056] Fig.21 It is a schematic diagram of Example 1 of the present invention after being subjected to a high temperature, high humidity and high pressure simulation experiment.
[0057] Fig. 22 It is a schematic diagram of comparative example 1 of the present invention after being subjected to a high temperature, high humidity and high pressure simulation experiment. DETAILED DESCRIPTION
[0058] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments, but the protection scope and implementation methods of the present invention are not limited thereto.
[0059] Unless otherwise specified, the materials and reagents used in the following examples are commercially available.
[0060] Solid content refers to the dry weight content of solids in water-based pressure-sensitive adhesives. Pressure-sensitive adhesive emulsions are generally composed of pressure-sensitive adhesive molecules, other additives and aqueous solutions. The solid content left after drying and removing water and other solvents is the solid content.
[0061] Example 1
[0062] A dispensing process comprises the following steps:
[0063] (1) 100 g of a water-based acrylic pressure-sensitive adhesive (brand name: MAC-100, 3M, the solid content of the water-based acrylic pressure-sensitive adhesive is 55%) is added to 895.5 g of deionized water, and magnetically stirred at room temperature for 20 min at a magnetic stirring speed of 500 rpm, and then 104.5 g of isopropyl alcohol is added dropwise while stirring, and stirring is continued for 10 min. After mixing evenly, a mixed solution is obtained, in which the solid content of the pressure-sensitive adhesive in the mixed solution is 5%;
[0064] (2) Add 5.5 g of Carbomer 940 (manufacturer: Lubrizol) to the mixed solution and continue stirring for 20 min to obtain a dispensing solution; the mass ratio of water to alcohol solvent in the dispensing solution is 9:1; the mass of Carbomer 940 is 0.5% of the mass of the mixed solution;
[0065] (3) The dispensing solution in step (2) is passed through Figure 1 The dispensing machine spray valve dispenses glue on the surface of PEN and the gas diffusion layer porous layer, and dries at room temperature for 20 minutes; the dispensing machine spray valve is provided with an external split mask structure (such as Figure 2 As shown), the mask structure is connected to the outside of the spray valve needle through a thread or a buckle, and a built-in slit is provided on the mask structure, and the width of the slit is 1 mm;
[0066] (4) Finally, the plasma-treated PEN and the GDL with the glue line in step (3) were pressed together at 0.2 MPa and room temperature for 15 seconds. The power of the plasma-treated PEN was 400 W, and the treatment time was 1 minute.
[0067] Example 2
[0068] A dispensing process comprises the following steps:
[0069] (1) 100 g of a water-based acrylic pressure-sensitive adhesive (brand name: MAC-100, 3M, the solid content of the water-based acrylic pressure-sensitive adhesive is 55%) is added to 131 g of deionized water, and magnetic stirring is performed at room temperature for 30 min at a magnetic stirring speed of 500 rpm. Then, 44 g of isopropanol is added dropwise while stirring, and stirring is continued for 30 min. After mixing evenly, a mixed solution is obtained, in which the solid content of the pressure-sensitive adhesive in the mixed solution is 20%;
[0070] (2) adding 0.275 g of Carbomer 940 (manufacturer: Lubrizol) to the mixed solution, and continuing stirring for 30 min to obtain a dispensing solution; the mass ratio of water to alcohol solvent in the dispensing solution is 8:2; the mass of Carbomer 940 is 0.1% of the mass of the mixed solution;
[0071] (3) The dispensing solution in step (2) is passed through Figure 1 The dispensing machine spray valve dispenses glue on the surface of PEN and the porous layer of the gas diffusion layer, and dries at room temperature for 20 minutes; the dispensing machine spray valve is provided with an external split mask structure, and the slit width of the mask structure is 1 mm;
[0072] (4) Finally, the plasma-treated PEN and the GDL with the glue line in step (3) were pressed together at 0.2 MPa and room temperature for 15 seconds. The power of the plasma-treated PEN was 400 W, and the treatment time was 1 minute.
[0073] Example 3
[0074] A dispensing process comprises the following steps:
[0075] (1) 100 g of a water-based acrylic pressure-sensitive adhesive (MAC-100, 3M, the solid content of the pressure-sensitive adhesive in the water-based acrylic pressure-sensitive adhesive is 55%) is added to 202.5 g of deionized water, and magnetic stirring is performed at room temperature for 20 min at a magnetic stirring speed of 500 rpm. Then, 247.5 g of ethanol is added dropwise while stirring, and stirring is continued for 20 min. After mixing evenly, a mixed solution is obtained, in which the solid content of the pressure-sensitive adhesive in the mixed solution is 10%;
[0076] (2) Add 1.65 g of Carbomer 940 (manufacturer: Lubrizol) to the mixed solution and continue stirring for 20 min to obtain a dispensing solution; the mass ratio of water to alcohol solvent in the dispensing solution is 5:5; the mass of Carbomer 940 is 0.3% of the mass of the mixed solution;
[0077] (3) The dispensing solution in step (2) is passed through Figure 1 The dispensing machine spray valve dispenses glue on the surface of PEN and the porous layer of the gas diffusion layer, and dries at room temperature for 20 minutes; the dispensing machine spray valve is provided with an external split mask structure, and the slit width of the mask structure is 1 mm;
[0078] (4) Finally, the plasma-treated PEN and the GDL with the glue line in step (3) were pressed together at 0.2 MPa and room temperature for 15 seconds. The power of the plasma-treated PEN was 400 W, and the treatment time was 1 minute.
[0079] Comparative Example 1:
[0080] A dispensing process comprises the following steps:
[0081] (1) A water-based acrylic pressure-sensitive adhesive (MAC-100, 3M, the solid content of the water-based acrylic pressure-sensitive adhesive is 55%) is dispensed on the surface of the PEN and the porous layer of the gas diffusion layer using a conventional dispenser spray valve (without a mask structure), and dried at room temperature for 20 minutes;
[0082] (2) The plasma-treated PEN and the GDL with the glue line in step (1) were pressed together at 0.2 MPa and room temperature for 15 seconds. The power of the plasma-treated PEN was 400 W and the treatment time was 1 minute.
[0083] Comparative Example 2:
[0084] A dispensing process comprises the following steps:
[0085] (1) 100 g of water-based acrylic pressure-sensitive adhesive (MAC-100, 3M, the solid content of the pressure-sensitive adhesive in the water-based acrylic pressure-sensitive adhesive is 55%) is added to 895.5 g of deionized water, and magnetically stirred at room temperature for 20 min at a magnetic stirring speed of 500 rpm, and then 104.5 g of isopropyl alcohol is added dropwise while stirring, and stirring is continued for 10 min to obtain a dispensing solution; the solid content of the pressure-sensitive adhesive in the dispensing solution is 5%; the mass ratio of water to alcohol solvent in the dispensing solution is 9:1;
[0086] (2) The dispensing solution in step (1) is passed through Figure 1 The dispensing machine sprays the glue on the surface of PEN and the porous layer of the gas diffusion layer, the slit width of the mask structure is 1 mm, and the glue is dried at room temperature for 20 minutes;
[0087] (3) Finally, the plasma-treated PEN and the GDL with the glue line in step (2) were pressed together at 0.2 MPa and room temperature for 15 seconds. The power of the plasma-treated PEN was 400 W, and the treatment time was 1 minute.
[0088] Comparative Example 3:
[0089] A dispensing process comprises the following steps:
[0090] (1) adding 100 g of a water-based acrylic pressure-sensitive adhesive (MAC-100, 3M, the solid content of the water-based acrylic pressure-sensitive adhesive being 55%) to 1000 g of deionized water, stirring the mixture by magnetic force at room temperature for 20 min at a speed of 500 rpm, and mixing the mixture to obtain a mixed solution, wherein the solid content of the pressure-sensitive adhesive in the mixed solution is 5%;
[0091] (2) Then, 5.5 g of Carbomer 940 (manufacturer: Lubrizol) was added to step (1), and stirring was continued for 20 min to obtain a dispensing solution; the mass of Carbomer 940 was 0.5% of the mass of the mixed solution;
[0092] (3) The dispensing solution in step (2) is passed through Figure 1 The dispensing machine sprays the glue on the surface of PEN and the porous layer of the gas diffusion layer, the slit width of the mask structure is 1 mm, and the glue is dried at room temperature for 20 minutes;
[0093] (4) Finally, the plasma-treated PEN and the GDL with the glue line in step (3) were pressed together at 0.2 MPa and room temperature for 15 seconds. The power of the plasma-treated PEN was 400 W, and the treatment time was 1 minute.
[0094] Comparative Example 4:
[0095] A dispensing process comprises the following steps:
[0096] (1) 100 g of a water-based acrylic pressure-sensitive adhesive (MAC-100, 3M, the solid content of the water-based acrylic pressure-sensitive adhesive is 55%) is added to 268.5 g of deionized water, and magnetically stirred at room temperature for 20 min at a magnetic stirring speed of 500 rpm, and then 731.5 g of isopropanol is added dropwise while stirring, and stirring is continued for 10 min. After mixing evenly, a mixed solution is obtained, in which the solid content of the pressure-sensitive adhesive in the mixed solution is 5%;
[0097] (2) Add 5.5 g of Carbomer 940 (manufacturer: Lubrizol) to the mixed solution and continue stirring for 20 min to obtain a dispensing solution; the mass ratio of water to alcohol solvent in the dispensing solution is 3:7; the mass of Carbomer 940 is 0.5% of the mass of the mixed solution;
[0098] (3) The dispensing solution in step (2) is passed through Figure 1 The dispensing machine sprays the glue on the surface of PEN and the porous layer of the gas diffusion layer, the slit width of the mask structure is 1 mm, and the glue is dried at room temperature for 20 minutes;
[0099] (4) Finally, the plasma-treated PEN and the GDL with the glue line in step (3) were pressed together at 0.2 MPa and room temperature for 15 seconds. The power of the plasma-treated PEN was 400 W, and the treatment time was 1 minute.
[0100] Comparative Example 5
[0101] The difference from Example 1 is that 11 g of Carbomer 940 (manufacturer: Lubrizol) is added in step (2), and its mass is 1% of the mass of the mixed solution; the other steps are the same as Example 1.
[0102] Comparative Example 6
[0103] A dispensing process comprises the following steps:
[0104] The difference from Example 1 is that in step (1), 8.96 g of deionized water and 1.04 g of isopropanol are added, and the solid content of the pressure-sensitive adhesive in the mixed solution is 50%. The other steps are the same as in Example 1.
[0105] Experiment 1:
[0106] The glue line thickness of the PEN samples with glue lines in the above Examples 1-3 and Comparative Examples 1-6 was measured. The results are shown in Table 1.
[0107] Experiment 2:
[0108] The GDL and PEN bonding samples of the above Examples 1-3 and Comparative Examples 1-6 were cut into strips with a width of 20 mm. The universal testing machine clamped PEN at one end and GDL at the other end to perform a shear peel test. The peel rate was 10 mm / min. The shear bonding strength between GDL and PEN was tested. The results are shown in Table 2.
[0109] Experiment 3:
[0110] The GDL and PEN bonding samples of the above Example 3 and Comparative Examples 1-6 were placed in a 4T press with pressure-sensitive paper for 10 seconds to observe the uniformity of pressure distribution. The results are shown in FIG. Figure 3-11 .
[0111] Experiment 4:
[0112] The width and profile of the rubber line on the surface of the gas diffusion layer in Examples 1-3 and Comparative Examples 1-6 were observed under a microscope. Figure 12-20 .
[0113] Experiment 5:
[0114] The GDL and PEN bonding samples of Example 1 and Comparative Example 1 were respectively placed in a fixture with a clamping pressure of 10 MPa. The fixture was placed in an environmental box at 85°C and 85% RH. After 1000 hours, the penetration of the adhesive line in the gas diffusion layer was observed. The results are shown in FIG. Figure 21-22 .
[0115] Table 1 Thickness of glue line on PEN substrate
[0116]
[0117] Table 2 GDL and PEN substrate bonding strength test
[0118]
[0119] According to Table 1, the thickness of the glue lines in Examples 1-3 is less than 15 μm, which is significantly less than the 35 μm of the conventional glue line in Comparative Example 1. In Comparative Examples 5 and 6, due to the excessive viscosity or high solid content of the glue solution, the thickness control is poor, resulting in a glue line thickness greater than 15 μm.
[0120] According to Table 2, in Examples 1-3, due to the appropriate alcohol-water ratio, the pressure-sensitive adhesive can quickly partially penetrate into the porous layer of the gas diffusion layer. At the same time, since the supporting material PEN is treated with plasma to enhance its surface energy, even when the thickness of the glue line is ultra-thin, the bonding force between GDL and PEN is equivalent to the bonding force between GDL and PEN in the conventional comparative example 1, which meets the bonding requirements of MEA for GDL and five-in-one membrane electrode. In comparative example 3, since the solvent is only water, the glue line is difficult to penetrate the surface of the super-hydrophobic porous layer of GDL. When the thickness of the glue line is significantly thinned, the bonding force between GDL and PEN is also significantly reduced. In comparative example 4, due to the high alcohol content in the glue solution, the glue solution is too quickly penetrated into the GDL, resulting in less residual adhesive on the surface of GDL and it is difficult to effectively bond GDL and PEN.
[0121] according to Figure 3-Figure 5 Examples 1 to 3 and Figure 6 Comparative Example 1 and Figure 10-11 From the pressure distribution of the glue line bonding area under pressure in Comparative Examples 5 and 6, it can be seen that there is no significant difference in pressure between the glue line of the present invention and the glue-free line, while the pressure at the glue line of the conventional gas diffusion layer glue-point bonding process is significantly higher than that in other areas. At the same time, when the glue line is too thick, it will also cause the problem of pressure concentration. This shows that the ultra-thin glue line process of the present invention can effectively solve the defects of the gas diffusion layer such as destructive cracks caused by excessive pressure.
[0122] The observation results of the glue lines of Examples 1-3, Comparative Example 1 and Comparative Example 2 under a microscope are as follows: Figure 12-20As shown in the glue line picture, examples 1-3 (see Figure 12-14 ) The glue line width is well controlled and the profile is uniform, while the comparative example 1 (see Fig.15 ) Because the conventional dispensing process is difficult to control, the glue line glue width is inaccurately controlled and the contour is uneven. Fig.16 ) Since no thickener is added, the viscosity of the dispensing solution is too low, and diffusion will occur on the GDL surface during the dispensing process, which also leads to inaccurate control of the glue line width and uneven contour. Figure 19-20 ) Due to excessive viscosity or high solid content, the thickness and uniformity of the glue line are difficult to control during the dispensing process, which is manifested as the glue line is too thick and the cutting width uniformity is poor.
[0123] According to the results of the high temperature, high humidity and high pressure simulation experiment of Example 1 and Comparative Example 1 ( Fig.21 and Fig. 22 As shown in the circle in the middle, since the thickness of the glue line in Comparative Example 1 is relatively thick, the pressure in the glue line area is significantly higher than that in other areas. Under the conditions of high temperature, high humidity and high pressure for a long time, the glue line penetrates into the porous GDL and even penetrates to the back of the GDL, which may affect the performance of the membrane electrode. However, since the thickness of the glue line is significantly reduced in Example 1, the pressure on it is significantly reduced. Therefore, it is difficult for the pressure-sensitive adhesive to penetrate the porous GDL in a high temperature and high humidity environment, thereby protecting the performance of the membrane electrode from being affected.
[0124] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A dispensing process, characterized in that: The following steps are involved: (1) diluting an aqueous pressure-sensitive adhesive emulsion with a mixed solvent of water and alcohol to obtain a mixed solution, wherein the pressure-sensitive adhesive solid content in the mixed solution is 5-40%; the aqueous pressure-sensitive adhesive emulsion is an aqueous acrylic pressure-sensitive adhesive; (2) adding a thickener to the mixed solution and mixing them uniformly to obtain a dispensing solution, wherein the mass ratio of water to the alcohol solvent in the dispensing solution is (9-5): (1-5), and the viscosity of the dispensing solution is 50-200 cp; (3) dispensing the dispensing solution obtained in step (2) on the surface of the gas diffusion layer using a dispensing machine, wherein an external split mask structure is provided below the spray valve on the dispensing machine, the mask structure is connected to the outside of the spray valve needle by a thread or a buckle, and the mask structure is also provided with a built-in slit; (4) Pressing the gas diffusion layer obtained in step (3) onto the membrane electrode support material; In step (1), the alcohol solvent is at least one of ethanol, propanol, butanol, ethylene glycol, ethoxyethanol, and methoxyethanol; The mass of the thickener in step (2) is 0.1-0.5% of the mass of the mixed solution.
2. The dispensing process according to claim 1, characterized in that: In the step (1), the mass ratio of the aqueous pressure-sensitive adhesive latex, water and alcohol is 1: (0.1-10): (0.1-5).
3. The dispensing process according to claim 1, characterized in that: The thickener in step (2) is at least one of carbomer resin, polyacrylic acid, and cellulose ether.
4. The dispensing process according to claim 1, characterized in that: In the step (3), the distance between the mask structure and the gas diffusion layer is 0.05-3 mm.
5. The dispensing process according to claim 1, characterized in that: The slit width of the mask structure in step (3) is 0.5-5 mm.
6. The dispensing process according to claim 1, characterized in that: In the step (4), the membrane electrode support material is pre-treated with plasma.
7. The dispensing process according to claim 1, characterized in that: In the step (4), the pressure when the gas diffusion layer and the membrane electrode support material are pressed is 0.05-0.3 MPa, and the pressing time is 5-30 s.
8. Application of the dispensing process as described in any one of claims 1 to 7 in fuel cell membrane electrode.