Wear-resistant plastic mold steel and preparation method thereof
By dispersing nano-ceramic particles in plastic mold steel and adopting multiple quenching processes, the problem of insufficient surface hardness of existing plastic mold steel is solved, achieving high-precision, low-cost wear resistance and excellent hardenability and polishing properties. .
Patent Information
- Application Number
- CN202311397013.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-10-26
AI Technical Summary
Existing plastic mold steels are difficult to meet the needs of high-precision plastic processing, especially the surface hardness in the annealed state is less than 300HBW, and Ni25Cr15Ti2MoMn and Ni53Cr19Mo3TiNb mold steels with high content of precious metal elements and high cost are not suitable for use in plastic molds.
Develop a wear-resistant plastic mold steel containing C, Si, Mn, Cr, Mo, Ni and other elements, and disperse nano-ceramic particles in it. Through quenching and tempering treatment, the proportion of tempered martensite exceeds 92%. , prepared by pressure casting and multiple quenching processes to ensure that the surface hardness reaches above 300HBW and the cost is relatively low.
It achieves wear resistance with a surface hardness of over 300HBW, excellent hardenability and polishing performance, low cost, and is suitable for the production of high-precision plastic molds.
Smart Images

Figure CN117403130B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of mold steel, and in particular to a wear-resistant plastic mold steel and a preparation method thereof. Background Art
[0002] As plastic products are used more and more widely in industry and daily life, the demand for mold steel in the plastic mold industry is also increasing. In plastic molding processing, the quality of the mold has a great impact on the quality of the product. The parts of plastic molds are divided into two categories: one is structural parts, including pouring systems, guides, top templates, ejector mechanisms, supports, etc.; the other is molded parts, including cavities, cores, inlays, etc. Among them, the first type of parts can be designed for strength and structure according to the requirements of mechanical parts, and the materials are generally selected from medium and low carbon structural steel, alloy steel and carbon steel. Due to the complex structure of the molded parts, the workpiece requires high dimensional accuracy, low surface roughness, and good joint tightness, which puts forward professional requirements for the mechanical properties, wear resistance and processing technology of the mold material.
[0003] The plastic mold steel currently used in my country is still mainly 4Cr13 mold steel, whose annealed surface hardness can reach 200HBW. After special heat treatment, its annealed surface hardness can reach 240HBW. It has excellent hardenability, good polishing performance and relatively low cost.
[0004] However, as the requirements for product precision in plastic processing are getting higher and higher, the requirements for mold steel are also increasing. Many precision plastic components require plastic mold steel with an annealed surface hardness of more than 300HBW to meet processing needs. However, in my country's current national standard GB / T 1299-2014 "Tool Steel", only two types of mold steel, Ni25Cr15Ti2MoMn and Ni53Cr19Mo3TiNb, can achieve the above hardness. However, the above two types of mold steel are mainly used for metal processing, have excellent hot processing performance, and are relatively expensive, and are not suitable for the preparation of plastic molds. Summary of the invention
[0005] In order to solve at least one of the above technical problems, a plastic mold steel with relatively low cost, high surface hardness in annealed state, excellent hardenability and good polishing performance is developed. The present application provides a wear-resistant plastic mold steel and a preparation method thereof.
[0006] On the one hand, the present application provides a wear-resistant plastic mold steel, wherein the mass fraction ratio of each component of the plastic mold steel is: C is 0.4~0.5%, Si is 0.1~0.4%, Mn is 0.2~0.5%, Cr is 1.2~1.5%, Mo is 0.1~0.2%, Ni is 3.8~4.2%, P content is not more than 0.05%, S content is not more than 0.05%, nano-ceramic particle content is 0.6~0.8%, and the balance is Fe; the nano-ceramic particles are dispersed in the plastic mold steel alloy, and the plastic mold steel is quenched and tempered, and the tempered martensite accounts for more than 92% in the metallographic structure.
[0007] Optionally, the nano-ceramic particles are nano-alumina and / or nano-zirconia ceramic particles.
[0008] Optionally, the particle size of the nano-ceramic particles is controlled to be 50-120 nm.
[0009] On the other hand, the present application also provides a method for preparing the above-mentioned wear-resistant plastic mold steel, comprising the following steps:
[0010] S1. According to the formula of nano-ceramic particles, the corresponding amount of nano-metal oxide and Ni powder are prepared into intermetallic compounds, and the addition amount of the remaining Ni element is calculated according to the formula of the alloying element, and the remaining Ni metal raw material is accurately weighed;
[0011] S2. According to the formula amount of the alloying elements, the remaining metal raw materials except the Ni element are melted into a liquid state at a high temperature, and the remaining Ni metal raw material weighed in step S1 is added to the molten metal obtained by melting to obtain a molten metal liquid;
[0012] S3, placing the intermetallic compound obtained in step S1 at the bottom of the ladle, and pouring the molten metal in step S2 into the ladle to obtain a molten alloy;
[0013] S4, casting the alloy liquid obtained in step S3 into the required mold steel blank by pressure casting;
[0014] S5. Heat the mold steel blank to 560-620°C in a vacuum furnace at a heating rate of 5-10°C / min, keep the temperature for more than 30 minutes, and then cool it naturally to room temperature;
[0015] S6, heating the mold steel blank after the treatment in step S5 to 440-480°C in a heating furnace at a heating rate of 3-5°C / min, and keeping the temperature for 10-15min; then heating the mold steel blank to 880-910°C at a heating rate of 8-12°C / min, and keeping the temperature for more than 1h; taking out the mold steel blank, quenching it with oil, and letting it stand to room temperature;
[0016] S7, repeat step S6 1 to 3 times;
[0017] S8, heating the mold steel blank after the treatment in step S7 to 420-460°C at a heating rate of 5-8°C / min, keeping the temperature for more than 30 minutes, and then naturally cooling to room temperature;
[0018] S9, machining, grinding and polishing the mold steel blank processed in step S8 to obtain a mold steel finished product.
[0019] By adopting the above technical scheme, the present application designs a medium-carbon alloy steel containing Mo and Cr elements with a relatively high Ni content, and dispersed nano-ceramic particles are dispersed therein. The tempered martensite content in the alloy is made to exceed 92% by heat treatment. The obtained mold steel has extremely high surface hardness, and the tempered surface hardness can reach more than 300HBW, and the wear resistance is extremely excellent; the mold steel of the present application has an extremely low content of Mo element and does not contain precious metal elements, the cost is relatively low, and the polishing performance and hardenability are relatively excellent.
[0020] Optionally, in step S1, corresponding amounts of nano-metal oxide and Ni powder are prepared into intermetallic compounds by the following steps: first, according to the amount of nano-metal oxide, the amount of corresponding metal element is calculated, and the nano-powder of the metal element corresponding to the nano-metal oxide is accurately weighed; then, the nano-powder of the metal element corresponding to the nano-metal oxide is mixed with the nano-powder of the Ni element, and the mixed powder is obtained by mechanical grinding for more than 30 minutes; finally, the mixed powder is heated in a heating furnace under low oxygen for 15 to 30 minutes to obtain an intermetallic compound.
[0021] Optionally, in step S2, the smelting temperature is controlled at 1600-1680°C.
[0022] Optionally, in step S3, after the molten metal is poured into the ladle, it is left to stand for 1 to 3 minutes.
[0023] Optionally, in step S5, the temperature is raised to 580-590°C.
[0024] Optionally, in step S6, the temperature is increased to 892-896° C. at a heating rate of 8-12° C. / min.
[0025] Optionally, in step S7, step S6 is repeated twice.
[0026] In summary, the present invention includes at least one of the following beneficial technical effects:
[0027] The present application designs a medium-carbon alloy steel containing Mo and Cr elements with a relatively high Ni content, and dispersed nano-ceramic particles are dispersed therein. The tempered martensite content in the alloy is made to exceed 92% through heat treatment. The obtained mold steel has extremely high surface hardness, and the tempered surface hardness can reach more than 300 HBW, and the wear resistance is extremely excellent.
[0028] The mold steel of the present application has an extremely low content of Mo element and does not contain precious metal elements, so the cost is relatively low, and the polishing performance and hardenability are relatively excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a 50μm electron microscope image of the plastic mold steel of Example 1 of the present application. Implementation
[0030] The present application is further described in detail below with reference to the embodiments.
[0031] The present application designs a wear-resistant plastic mold steel, wherein the mass fraction ratio of each component of the plastic mold steel is: C is 0.4-0.5%, Si is 0.1-0.4%, Mn is 0.2-0.5%, Cr is 1.2-1.5%, Mo is 0.1-0.2%, Ni is 3.8-4.2%, P content is not more than 0.05%, S content is not more than 0.05%, nano-ceramic particle content is 0.6-0.8%, and the balance is Fe; the nano-ceramic particles are dispersed in the plastic mold steel alloy, and the plastic mold steel is quenched and tempered, and the tempered martensite accounts for more than 92% in the metallographic structure.
[0032] In order to obtain the above metallographic structure of the present application, the wear-resistant plastic mold steel of the present application is prepared by the following steps:
[0033] S1. According to the formula of nano-ceramic particles, the corresponding amount of nano-metal oxide and Ni powder are prepared into intermetallic compounds, and the addition amount of the remaining Ni element is calculated according to the formula of the alloying element, and the remaining Ni metal raw material is accurately weighed;
[0034] S2. According to the formula amount of the alloying elements, the remaining metal raw materials except the Ni element are melted into a liquid state at a high temperature, and the remaining Ni metal raw material weighed in step S1 is added to the molten metal obtained by melting to obtain a molten metal liquid;
[0035] S3, placing the intermetallic compound obtained in step S1 at the bottom of the ladle, and pouring the molten metal in step S2 into the ladle to obtain a molten alloy;
[0036] S4, casting the alloy liquid obtained in step S3 into the required mold steel blank by pressure casting;
[0037] S5. Heat the mold steel blank to 560-620°C in a vacuum furnace at a heating rate of 5-10°C / min, keep the temperature for more than 30 minutes, and then cool it naturally to room temperature;
[0038] S6, heating the mold steel blank after the treatment in step S5 to 440-480°C in a heating furnace at a heating rate of 3-5°C / min, and keeping the temperature for 10-15min; then heating the mold steel blank to 880-910°C at a heating rate of 8-12°C / min, and keeping the temperature for more than 1h; taking out the mold steel blank, quenching it with oil, and letting it stand to room temperature;
[0039] S7, repeat step S6 1 to 3 times;
[0040] S8, heating the mold steel blank after the treatment in step S7 to 420-460°C at a heating rate of 5-8°C / min, keeping the temperature for more than 30 minutes, and then naturally cooling to room temperature;
[0041] S9, machining, grinding and polishing the mold steel blank processed in step S8 to obtain a mold steel finished product.
[0042] Among them, the metal oxide particles and Ni of the present application are preferably prepared into intermetallic compounds by the following method:
[0043] Firstly, the amount of the corresponding metal element is calculated according to the amount of the nano-metal oxide, and the nano-powder of the metal element corresponding to the nano-metal oxide is accurately weighed; then, the nano-powder of the metal element corresponding to the nano-metal oxide is mixed with the nano-powder of the Ni element, and the mixed powder is obtained by mechanical grinding for more than 30 minutes; finally, the mixed powder is heated in a heating furnace under low oxygen for 15 to 30 minutes to obtain an intermetallic compound.
[0044] The above method is used to prepare nano-metal oxide particles and Ni to prepare intermetallic compounds. Not only are the raw materials easy to obtain, but the corresponding nano-mixed powders of metal elements and Ni elements can be directly purchased from the market. The preparation process is simple and the quality of the obtained intermetallic compounds is very excellent.
[0045] The following are preparation examples and embodiments of the present application.
[0046] The inventor of the present application has conducted experiments and found that the alloy formula of the present application is adopted and the ratio of the alloy elements is adjusted within the formula, which has a very small impact on the performance of the plastic mold steel finally obtained by the present application.
[0047] Therefore, the embodiments of the present application uniformly adopt the following formula: C is 0.45%, Si is 0.3%, Mn is 0.4%, Cr is 1.4%, Mo is 0.15%, Ni is 3.8%, P content is not more than 0.05%, S content is not more than 0.05%, nano-ceramic particle content is 0.8%, and the balance is Fe.
[0048] In addition, the nano-ceramic particles of the present application can be prepared from ceramic particles such as nano-alumina, nano-zirconia or nano-yttrium oxide, or mixed particles of the above ceramic particles, and the alloy of the present application has excellent properties. For the convenience of experiment, the present application example uses nano-alumina ceramic particles.
[0049] The sources of raw materials for each part of the examples of this application are as follows:
[0050] The main raw materials of this application are scrap steel purchased from the market; Mn ingots, Cr plates, Ni ingots, and Mo bars are all purchased from Hebei Fengchu Metal Materials Trading Co., Ltd.; Si powder is purchased from Shanghai Buwei Applied Materials Technology Co., Ltd.; and nickel-aluminum alloy nanopowder is purchased from Shanghai Jingyan Chemical Technology Co., Ltd.
[0051] The following is an example of the preparation of an alumina-Ni intermetallic compound.
[0052] Preparation Example 1
[0053] This preparation example uses a nickel-aluminum alloy nanopowder with an aluminum-nickel mass ratio of 1:1 and a particle size of 120 nm.
[0054] S1-1. Calculate the amount of aluminum element according to the amount of nano-alumina ceramic particles added in the alloy formula, and then accurately weigh the nickel-aluminum alloy nanopowder according to the calculated result;
[0055] S1-2, grinding the nickel-aluminum alloy nanopowder with a ball mill for 30 minutes;
[0056] S1-3. Put the nickel-aluminum alloy nanopowder that has been mechanically ground into a heating furnace, introduce a low-oxygen atmosphere, control the temperature at 620-680°C, and heat for 30 minutes to obtain alumina-Ni intermetallic compound nanopowder.
[0057] The low oxygen atmosphere is an atmosphere in which the volume ratio of air to pure nitrogen is 1:1.
[0058] Preparation Example 2
[0059] This preparation example uses nickel-aluminum alloy nanopowder with an aluminum-nickel mass ratio of 1:1 and a particle size of 100 nm.
[0060] S1-1. Calculate the amount of aluminum element according to the amount of nano-alumina ceramic particles added in the alloy formula, and then accurately weigh the nickel-aluminum alloy nanopowder according to the calculated result;
[0061] S1-2, grinding the nickel-aluminum alloy nanopowder with a ball mill for 30 minutes;
[0062] S1-3. Put the nickel-aluminum alloy nanopowder that has been mechanically ground into a heating furnace, introduce a low-oxygen atmosphere, control the temperature at 620-680°C, and heat for 25 minutes to obtain alumina-Ni intermetallic compound nanopowder.
[0063] The low oxygen atmosphere is an atmosphere in which the volume ratio of air to pure nitrogen is 1:1.
[0064] Preparation Example 3
[0065] This preparation example uses nickel-aluminum alloy nanopowder with an aluminum-nickel mass ratio of 1:1 and a particle size of 80 nm.
[0066] S1-1. Calculate the amount of aluminum element according to the amount of nano-alumina ceramic particles added in the alloy formula, and then accurately weigh the nickel-aluminum alloy nanopowder according to the calculated result;
[0067] S1-2, grinding the nickel-aluminum alloy nanopowder by a ball mill for 40 minutes;
[0068] S1-3. Put the nickel-aluminum alloy nanopowder that has been mechanically ground into a heating furnace, introduce a low-oxygen atmosphere, control the temperature at 620-680°C, and heat for 20 minutes to obtain alumina-Ni intermetallic compound nanopowder.
[0069] The low oxygen atmosphere adopts an atmosphere in which the volume ratio of air and pure nitrogen is 1:1.2.
[0070] Preparation Example 4
[0071] This preparation example uses nickel-aluminum alloy nanopowder with an aluminum-nickel mass ratio of 1:1 and a particle size of 50 nm.
[0072] S1-1. Calculate the amount of aluminum element according to the amount of nano-alumina ceramic particles added in the alloy formula, and then accurately weigh the nickel-aluminum alloy nanopowder according to the calculated result;
[0073] S1-2, grinding the nickel-aluminum alloy nanopowder by a ball mill for 45 minutes;
[0074] S1-3. Put the nickel-aluminum alloy nanopowder that has been mechanically ground into a heating furnace, introduce a low-oxygen atmosphere, control the temperature at 620-680°C, and heat for 15 minutes to obtain alumina-Ni intermetallic compound nanopowder.
[0075] The low oxygen atmosphere adopts an atmosphere in which the volume ratio of air and pure nitrogen is 1:1.2.
[0076] Preparation Example 5
[0077] This preparation example uses nickel-aluminum alloy nanopowder with an aluminum:nickel ratio of 1:1 and a particle size of 30 nm.
[0078] S1-1. Calculate the amount of aluminum element according to the amount of nano-alumina ceramic particles added in the alloy formula, and then accurately weigh the nickel-aluminum alloy nanopowder according to the calculated result;
[0079] S1-2, grinding the nickel-aluminum alloy nanopowder by a ball mill for 45 minutes;
[0080] S1-3. Put the nickel-aluminum alloy nanopowder that has been mechanically ground into a heating furnace, introduce a low-oxygen atmosphere, control the temperature at 620-680°C, and heat for 15 minutes to obtain alumina-Ni intermetallic compound nanopowder.
[0081] The low oxygen atmosphere adopts an atmosphere in which the volume ratio of air to pure nitrogen is 1:1.5.
[0082] The following is an example of the preparation of the alloy steel blank of the present application.
[0083] Preparation Example 6
[0084] The wear-resistant plastic mold steel blank of this preparation example is prepared by the following steps:
[0085] S1, using the aluminum oxide-Ni intermetallic compound nanopowder of Preparation Example 3; calculating the amount of the remaining Ni element except the Ni element occupied in the aluminum oxide-Ni intermetallic compound nanopowder according to the alloy formula, and cutting the Ni ingot raw material into Ni blocks, accurately weighing and setting aside;
[0086] S2. Calculate the amount of metal raw materials according to the formula, accurately weigh the scrap steel according to the calculation result, and cut the Mn ingot, Cr block and Mo bar into small pieces and accurately weigh them; except for the Ni element, put the accurately weighed metal raw materials into the smelting furnace, control the smelting temperature at 1600-1680° C., and melt them into liquid, and then put the Ni block weighed in step S1 into the smelting furnace to obtain molten metal;
[0087] S3, placing alumina-Ni intermetallic compound nanopowder at the bottom of the ladle, and then pouring the molten metal in step S2 into the ladle to obtain a molten alloy;
[0088] S4, directly subjecting the alloy liquid obtained in step S3 to pressure casting to form the required mold steel blank.
[0089] Preparation Example 7
[0090] The wear-resistant plastic mold steel blank of this preparation example is prepared by the following steps:
[0091] S1, using the aluminum oxide-Ni intermetallic compound nanopowder of Preparation Example 3; calculating the amount of the remaining Ni element except the Ni element occupied in the aluminum oxide-Ni intermetallic compound nanopowder according to the alloy formula, and cutting the Ni ingot raw material into Ni blocks, accurately weighing and setting aside;
[0092] S2. Calculate the amount of metal raw materials according to the formula, accurately weigh the scrap steel according to the calculation result, and cut the Mn ingot, Cr block and Mo bar into small pieces and accurately weigh them; except for the Ni element, put the accurately weighed metal raw materials into the smelting furnace, control the smelting temperature at 1600-1680° C., and melt them into liquid, and then put the Ni block weighed in step S1 into the smelting furnace to obtain molten metal;
[0093] S3, placing alumina-Ni intermetallic compound nanopowder at the bottom of the ladle, and then pouring the molten metal in step S2 into the ladle, and letting it stand for 1 minute to obtain a molten alloy;
[0094] S4: The alloy liquid obtained in step S3 is directly pressure cast to form the required mold steel blank.
[0095] Preparation Example 8
[0096] The wear-resistant plastic mold steel blank of this preparation example is prepared by the following steps:
[0097] S1, using the aluminum oxide-Ni intermetallic compound nanopowder of Preparation Example 3; calculating the amount of the remaining Ni element except the Ni element occupied in the aluminum oxide-Ni intermetallic compound nanopowder according to the alloy formula, and cutting the Ni ingot raw material into Ni blocks, accurately weighing and setting aside;
[0098] S2. Calculate the amount of metal raw materials according to the formula, accurately weigh the scrap steel according to the calculation result, and cut the Mn ingot, Cr block and Mo bar into small pieces and accurately weigh them; except for the Ni element, put the accurately weighed metal raw materials into the smelting furnace, control the smelting temperature at 1600-1680° C., and melt them into liquid, and then put the Ni block weighed in step S1 into the smelting furnace to obtain molten metal;
[0099] S3, placing alumina-Ni intermetallic compound nanopowder at the bottom of the ladle, and then pouring the molten metal in step S2 into the ladle, and letting it stand for 2 minutes to obtain a molten alloy;
[0100] S4: The alloy liquid obtained in step S3 is directly pressure cast to form the required mold steel blank.
[0101] Preparation Example 9
[0102] The wear-resistant plastic mold steel blank of this preparation example is prepared by the following steps:
[0103] S1, using the aluminum oxide-Ni intermetallic compound nanopowder of Preparation Example 3; calculating the amount of the remaining Ni element except the Ni element occupied in the aluminum oxide-Ni intermetallic compound nanopowder according to the alloy formula, and cutting the Ni ingot raw material into Ni blocks, accurately weighing and setting aside;
[0104] S2. Calculate the amount of metal raw materials according to the formula, accurately weigh the scrap steel according to the calculation result, and cut the Mn ingot, Cr block and Mo bar into small pieces and accurately weigh them; except for the Ni element, put the accurately weighed metal raw materials into the smelting furnace, control the smelting temperature at 1600-1680° C., and melt them into liquid, and then put the Ni block weighed in step S1 into the smelting furnace to obtain molten metal;
[0105] S3, placing alumina-Ni intermetallic compound nanopowder at the bottom of the ladle, and then pouring the molten metal in step S2 into the ladle, and letting it stand for 3 minutes to obtain a molten alloy;
[0106] S4: The alloy liquid obtained in step S3 is directly pressure cast to form the required mold steel blank.
[0107] The following are Examples 1 to 5 of the present application. Example
[0108] The wear-resistant plastic mold steel of this preparation example is prepared by the following steps:
[0109] S5. Using the mold steel blank of Preparation Example 8, heating it to 560° C. at a heating rate of 5° C. / min in a vacuum furnace, keeping it at that temperature for 60 min, and then naturally cooling it to room temperature;
[0110] S6, heating the mold steel blank treated in step S5 to 440°C in a heating furnace at a heating rate of 5°C / min, and keeping the temperature for 10 minutes; then heating it to 880°C at a heating rate of 8°C / min, and keeping the temperature for 1 hour; taking it out, oil quenching it, and letting it stand to room temperature;
[0111] S7, repeat step S6 twice;
[0112] S8, heating the mold steel blank after the treatment in step S7 to 420°C at a heating rate of 5°C / min, keeping the temperature for 30 minutes, and then naturally cooling to room temperature;
[0113] S9, machining, grinding and polishing the mold steel blank processed in step S8 to obtain a mold steel finished product. Example
[0114] The wear-resistant plastic mold steel of this embodiment is prepared by the following steps:
[0115] S5. Using the mold steel blank of Preparation Example 8, heating it to 620°C at a heating rate of 10°C / min in a vacuum furnace, keeping it at this temperature for more than 30 minutes, and then naturally cooling it to room temperature;
[0116] S6, heating the mold steel blank treated in step S5 to 480°C in a heating furnace at a heating rate of 3°C / min, and keeping the temperature for 15 minutes; then heating it to 910°C at a heating rate of 12°C / min, and keeping the temperature for 1 hour; taking it out, oil quenching it, and letting it stand to room temperature;
[0117] S7, repeat step S6 once;
[0118] S8, heating the mold steel blank after the treatment in step S7 to 460°C at a heating rate of 8°C / min, keeping the temperature for more than 30 minutes, and then naturally cooling to room temperature;
[0119] S9, machining, grinding and polishing the mold steel blank processed in step S8 to obtain a mold steel finished product. Example
[0120] The wear-resistant plastic mold steel of this embodiment is prepared by the following steps:
[0121] S5. Using the mold steel blank of Preparation Example 8, heating it to 590° C. at a heating rate of 8° C. / min in a vacuum furnace, keeping it at that temperature for 30 min, and then naturally cooling it to room temperature;
[0122] S6, heating the mold steel blank treated in step S5 to 460°C in a heating furnace at a heating rate of 5°C / min, and keeping the temperature for 15 minutes; then heating it to 890°C at a heating rate of 10°C / min, and keeping the temperature for 1 hour; taking it out, oil quenching it, and letting it stand to room temperature;
[0123] S7, repeat step S6 twice;
[0124] S8, heating the mold steel blank after the treatment in step S7 to 440°C at a heating rate of 8°C / min, keeping the temperature for 30 minutes, and then naturally cooling to room temperature;
[0125] S9, machining, grinding and polishing the mold steel blank processed in step S8 to obtain a mold steel finished product. Example
[0126] S5. Using the mold steel blank of Preparation Example 8, heating it to 590° C. at a heating rate of 8° C. / min in a vacuum furnace, keeping it at that temperature for 30 min, and then naturally cooling it to room temperature;
[0127] S6, heating the mold steel blank treated in step S5 to 460°C in a heating furnace at a heating rate of 5°C / min, and keeping the temperature for 15 minutes; then heating it to 892°C at a heating rate of 10°C / min, and keeping the temperature for 1 hour; taking it out, quenching it with oil, and letting it stand to room temperature;
[0128] S7, repeat step S6 once;
[0129] S8, heating the mold steel blank after the treatment in step S7 to 440°C at a heating rate of 8°C / min, keeping the temperature for 30 minutes, and then naturally cooling to room temperature;
[0130] S9, machining, grinding and polishing the mold steel blank processed in step S8 to obtain a mold steel finished product. Example
[0131] The wear-resistant plastic mold steel of this embodiment is prepared by the following steps:
[0132] S5. Using the mold steel blank of Preparation Example 8, heating it to 590° C. at a heating rate of 8° C. / min in a vacuum furnace, keeping it at that temperature for 30 min, and then naturally cooling it to room temperature;
[0133] S6, heating the mold steel blank treated in step S5 to 460°C in a heating furnace at a heating rate of 5°C / min, and keeping the temperature for 15 minutes; then heating it to 894°C at a heating rate of 10°C / min, and keeping the temperature for 1 hour; taking it out, oil quenching it, and letting it stand to room temperature;
[0134] S7, repeat step S6 once;
[0135] S8, heating the mold steel blank after the treatment in step S7 to 440°C at a heating rate of 8°C / min, keeping the temperature for 30 minutes, and then naturally cooling to room temperature;
[0136] S9, machining, grinding and polishing the mold steel blank processed in step S8 to obtain a mold steel finished product.
[0137] Performance testing:
[0138] The test adopts the method recorded in the national standard GB / T 1299-2014 "Tool Steel".
[0139] Taking two types of mold steels with grades of Ni25Cr15Ti2MoMn and Ni53Cr19Mo3TiNb as comparative examples 1 and 2, the metallographic structure, hardenability and surface hardness of the plastic mold steels of Examples 1 to 5 of the present application and the mold steels of comparative examples 1 to 2 were tested respectively, and the results are shown in Table 1.
[0140] Table 1 Performance test results of Examples 1 to 5
[0141] Metallographic structure Hardenability (850℃, mm) Surface annealing hardness (HBW) Example 1 Tempered martensite accounts for 92% 4.8 321 Example 2 Tempered martensite accounts for 93% 4.6 318 Example 3 Tempered martensite accounts for 95% 4.7 332 Example 4 Tempered martensite accounts for 96% 4.7 338 Example 5 Tempered martensite accounts for 95% 4.7 326 Comparative Example 1 Ferrite + alloy hardening phase 2.1 296 Comparative Example 2 Ferrite + alloy hardening phase 2.3 298
[0142] It can be seen from the data in Table 1 that the plastic mold steels of Examples 1 to 5 of the present application have a metallographic structure dominated by tempered martensite, a small amount of dispersed ceramic particle strengthening points, and excellent hardenability. At a temperature of 850°C, the hardening depth can reach more than 4.5 mm, far exceeding the mold steels of Comparative Examples 1 and 2. In addition, the surface annealing hardness of the plastic mold steels of Examples 1 to 5 of the present application can reach about 320 HBW, which is higher than the mold steels of Comparative Examples 1 and 2.
[0143] According to the national standard GB / T 1299-2014 "Tool Steel", the mold steels of Comparative Examples 1 and 2 are mold steels used for high-temperature hot forging and hot extrusion molds, rather than plastic mold steels. The plastic mold steels of Examples 1 to 5 of the present application can exceed the mold steels of Comparative Examples 1 and 2 in terms of surface hardness parameters, which shows that the performance is very excellent.
[0144] It can also be seen from the data in Table 1 that the material hardness is optimal after adopting a specific preheating process and a specific quenching process in this application.
[0145] This test randomly selected the plastic mold steel of Example 1 and performed electron microscope scanning to verify the test results of the metallographic structure. The electron microscope scanning diagram is as follows: Figure 1 As shown. Figure 1 As shown, the plastic mold steel of Example 1 of the present application has a metallographic structure mainly composed of needle-shaped tempered martensite, with a small amount of ceramic particle hardening points dispersed therein.
[0146] The following are Examples 6 to 14 of the present application, which are based on Example 4 of the present application, using the same preparation method and element ratio, with only some differences. Example
[0147] The difference between this embodiment and embodiment 4 is that the die steel blank of preparation example 6 is used. Example
[0148] The difference between this embodiment and embodiment 4 is that the die steel blank of preparation example 7 is used. Example
[0149] The difference between this embodiment and embodiment 4 is that the die steel blank of preparation example 9 is used. Example
[0150] The difference between this embodiment and embodiment 4 is that the aluminum oxide-Ni intermetallic compound nanopowder of preparation example 1 is used. Example
[0151] The difference between this embodiment and embodiment 4 is that the aluminum oxide-Ni intermetallic compound nanopowder of preparation example 2 is used. Example
[0152] The difference between this embodiment and embodiment 4 is that the aluminum oxide-Ni intermetallic compound nanopowder of preparation example 4 is used. Example
[0153] The difference between this embodiment and embodiment 4 is that the aluminum oxide-Ni intermetallic compound nanopowder of preparation example 5 is used. Example
[0154] The difference between this embodiment and embodiment 4 is that in step S7, step S6 is repeated twice. Example
[0155] The difference between this embodiment and embodiment 4 is that in step S7, step S6 is repeated three times.
[0156] Performance testing:
[0157] The surface hardness of the plastic mold steels of Examples 6 to 14 of the present application was tested, and the results are shown in Table 2.
[0158] Table 2 Performance test results of Examples 6 to 14
[0159] Surface annealing hardness (HBW) Example 6 295 Example 7 316 Example 8 333 Example 9 319 Example 10 331 Embodiment 11 329 Example 12 308 Embodiment 13 344 Embodiment 14 346
[0160] It can be seen from the data in Table 2 that the control of the standing time after the molten metal is poured into the ladle is more critical. If casting is performed directly, the hardness of the obtained mold steel will drop significantly. If the standing time is too long, the hardness of the obtained mold steel will also drop significantly. The inventor speculates that this is related to the dispersibility of the ceramic particles. After the molten metal is poured into the ladle, it needs to be left standing for a certain period of time so that the intermetallic compounds are evenly dispersed in the molten metal due to the high temperature. The time should not be too short or too long. If the time is too short, it will lead to uneven dispersion; if the time is too long, it will cause the ceramic particles to float in the molten metal.
[0161] It can also be seen from the data in Table 2 that the intermetallic compound of the present application uses raw materials with a particle size of 80-100 nm, and the surface annealing hardness of the alloy obtained is optimal. The inventor speculates that the particle size of the ceramic reinforcement particles has a great influence on the performance of the alloy. If the particle size is too small, the alloy cannot be effectively strengthened, and if the particle size is too large, the internal stress of the alloy may exceed the limit, thereby causing the hardness of the alloy to decrease.
[0162] It can also be seen from the data in Table 2 that the present application can also use zirconium oxide ceramic particles, which can also enable the alloy to obtain a surface annealing hardness of 300 HBW. Using alumina ceramic particles, the surface annealing hardness of the alloy is better than that of zirconium oxide ceramic particles.
[0163] In addition, by comparing the data of Examples 13 and 14 of the present application and Example 4, it can be seen that the surface annealing hardness of the alloy of the present application can be further significantly improved after three quenchings, while the surface annealing hardness improvement is not obvious after four quenchings. The inventor speculates that after three quenching treatments, the tempered martensite accounts for the largest proportion in the metallographic structure of the alloy, and the ceramic particles can better form strengthening points of the hardening phase on the surface of the alloy, thereby improving the surface annealing hardness of the alloy; and after three quenchings, the metallographic structure of the alloy has been basically finalized, and further quenching has little effect on the metallographic structure of the alloy.
[0164] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A wear-resistant plastic mold steel, It is characterized in that The mass fraction ratio of each component of the plastic mold steel is: C is 0.4-0.5%, Si is 0.1-0.4%, Mn is 0.2-0.5%, Cr is 1.2-1.5%, Mo is 0.1-0.2%, Ni is 3.8-4.2%, P content is not more than 0.05%, S content is not more than 0.05%, nano-ceramic particle content is 0.6-0.8%, and the balance is Fe; the nano-ceramic particles are dispersed in the plastic mold steel alloy, and the particle size of the nano-ceramic particles is 50-120nm; the plastic mold steel is quenched and tempered, and the tempered martensite accounts for more than 92% in the metallographic structure.
2. The wear-resistant plastic mold steel according to claim 1, It is characterized in that The nano ceramic particles are nano alumina and / or nano zirconium oxide ceramic particles.
3. The wear-resistant plastic mold steel according to claim 1, It is characterized in that The particle size of the nano ceramic particles is controlled at 80-100 nm.
4. A method for preparing the wear-resistant plastic mold steel as claimed in claim 1, It is characterized in that The following steps are involved: S1. According to the formula of nano-ceramic particles, the corresponding amount of nano-metal oxide and Ni powder are prepared into intermetallic compounds, and the addition amount of the remaining Ni element is calculated according to the formula of the alloying element, and the remaining Ni metal raw material is accurately weighed; S2. According to the formula amount of the alloying elements, the remaining metal raw materials except the Ni element are melted into a liquid state at a high temperature, and the remaining Ni metal raw material weighed in step S1 is added to the molten metal obtained by melting to obtain a molten metal liquid; S3, placing the intermetallic compound obtained in step S1 at the bottom of the ladle, pouring the molten metal in step S2 into the ladle, and letting it stand for 1 to 3 minutes to obtain a molten alloy; S4, casting the alloy liquid obtained in step S3 into the required mold steel blank by pressure casting; S5. Heat the mold steel blank to 560-620°C in a vacuum furnace at a heating rate of 5-10°C / min, keep the temperature for more than 30 minutes, and then cool it naturally to room temperature; S6, heating the mold steel blank after the treatment in step S5 to 440-480°C in a heating furnace at a heating rate of 3-5°C / min, and keeping the temperature for 10-15min; then heating the mold steel blank to 880-910°C at a heating rate of 8-12°C / min, and keeping the temperature for more than 1h; taking out the mold steel blank, quenching it with oil, and letting it stand to room temperature; S7, repeat step S6 1 to 3 times; S8, heating the mold steel blank after the treatment in step S7 to 420-460°C at a heating rate of 5-8°C / min, keeping the temperature for more than 30 minutes, and then naturally cooling to room temperature; S9, machining, grinding and polishing the mold steel blank processed in step S8 to obtain a mold steel finished product.
5. The method for preparing the wear-resistant plastic mold steel according to claim 4, It is characterized in that In the step S1, corresponding amounts of nano-metal oxide and Ni powder are prepared into an intermetallic compound by the following steps: first, according to the amount of nano-metal oxide, the amount of the corresponding metal element is calculated, and the nano-powder of the metal element corresponding to the nano-metal oxide is accurately weighed; then, the nano-powder of the metal element corresponding to the nano-metal oxide is mixed with the nano-powder of the Ni element, and the mixed powder is obtained by mechanical grinding for more than 30 minutes; finally, the mixed powder is heated in a heating furnace under low oxygen for 15 to 30 minutes to obtain the intermetallic compound.
6. The method for preparing the wear-resistant plastic mold steel according to claim 4, It is characterized in that In step S2, the smelting temperature is controlled at 1600-1680°C.
7. The method for preparing the wear-resistant plastic mold steel according to claim 4, It is characterized in that In step S5, the temperature is raised to 580-590°C.
8. The method for preparing the wear-resistant plastic mold steel according to claim 4, It is characterized in that In the step S6, the temperature is increased to 892-896° C. at a heating rate of 8-12° C. / min.
9. The method for preparing the wear-resistant plastic mold steel according to claim 4, It is characterized in that In the step S7, step S6 is repeated twice.
Citation Information
Patent Citations
High-modulus low-temperature-tempered Al-containing alloy steel and preparation method
CN106048448A
Ultrahigh-wear-resistance high-toughness hot work die steel and preparation method thereof
CN114318124A