A high-strength high-temperature oxidation-resistant grate bar and a preparation method thereof

By preparing high-content chromium alloy materials, the problem of easy oxidation and wear of grate bars under high temperature conditions is solved, the oxidation resistance and high temperature strength are improved, the use cycle is extended and the cost is reduced, and more efficient use of grate bars is achieved.

CN117428153BActive Publication Date: 2024-11-15SHANXI JINHONG INNOVATION TECHNOLOGY CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202311324541.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-13
Publication Date
2024-11-15
Estimated Expiration
2043-10-13

AI Technical Summary

Technical Problem

The existing grate bars are prone to oxidation, wear and deform under high temperature conditions, resulting in a short service life and need to be replaced frequently, which affects the production efficiency and cost of the sintering machine.

Method used

Using the preparation method of high-strength anti-high temperature oxidation grate strips, by preparing coated sand for shell core, adding specific proportions of scrap steel, ferrochromium, nickel plate, ferromolybdenum and other materials, performing high-temperature melting and deoxygenation treatment, and adding calcium silicide and aluminum Elements such as silk form high-content chromium alloy materials, reduce carbon content, improve oxidation resistance and high temperature strength.

Benefits of technology

It significantly improves the oxidation resistance and high temperature strength of the alloy, extends the service cycle, reduces material costs, and has better use effect than conventional high-chrome cast iron grate bars, with a service cycle of up to 3 to 5 years.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117428153B_ABST
    Figure CN117428153B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of new metal materials, in particular to a high-strength high-temperature oxidation-resistant grate bar and a preparation method thereof. In the present invention, the chromium content in the alloy reaches 24-27%, and the carbon content is controlled at 0.2-0.5%, which effectively prevents the formation of chromium carbide (Cr) due to the reaction between carbon and chromium in the alloy. 3 C 2 ), avoiding the occurrence of chromium depletion, so the obtained alloy has higher oxidation resistance and high temperature strength. In addition, the present invention reduces the amount of precious metal nickel by adding niobium and vanadium elements through the microalloying method, but at the same time ensures that its performance is equivalent to that of an alloy material with a nickel content of 20%, greatly reducing material costs, improving high temperature strength, high temperature oxidation resistance, and high temperature corrosion resistance, and the service life can reach 3 to 5 years.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new metal materials, in particular to a high-strength high-temperature oxidation-resistant grate bar and a preparation method thereof. Background Art

[0002] The grate is the main part of the sintering machine trolley. The grate forms a trough-shaped space with the trolley railing to accommodate and carry the ore. The part of the grate that contacts the ore is the upper surface. The upper part of the grate is stressed and plays a supporting role. The bottom of the grate has two functions. First, it fixes the grate when turning over and unloading, so that it cannot fall off; second, it plays a supporting role when the top of the grate is under pressure, which can effectively prevent the grate from bending.

[0003] Before sintering, the sintering machine trolley adds ore at the head position, and the grate bars are impacted and worn by the ore. At this time, the temperature of the grate bars is the lowest. When the machine is started for the first time, the temperature of the grate bars is room temperature. During the sintering process, the grate bars move forward at a certain speed with the trolley. When the trolley reaches the tail of the machine, the ore is burned through. At this time, the temperature of the grate bars is the highest, which can reach more than 900°C. The grate bars are oxidized by the air under high temperature conditions. When the trolley is turned over to unload, the grate bars are worn by the high temperature of the ore. When the grate bars are exposed to the air, they are in a high-temperature tempering state. After repeated cycles of heating, cooling, impact, and wear, the grate bars are gradually oxidized, worn, deformed, and damaged.

[0004] Grate bars are vulnerable parts due to their harsh working conditions and complex reasons for damage. Replacing grate bars requires a lot of time, manpower and material resources. The service life of grate bars directly affects the production efficiency of sintering machines and the production cost of ore sintering. With the increase in the annual output of ore sintering in my country, the consumption of grate bars has also gradually increased. Therefore, it is very necessary for the metallurgical industry to develop grate bar products with good use effect and low production cost. Summary of the invention

[0005] The object of the present invention is to provide a high-strength high-temperature oxidation-resistant grate bar and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a high-strength high-temperature oxidation-resistant grate bar and a preparation method thereof, comprising the following steps:

[0007] Step 1: Prepare coated sand for shell core:

[0008] The coated sand is heated, solidified, and sand-shot to obtain a coated sand shell mold, the surface of the coated sand shell mold is infiltrated with a water-based coating, and the shell mold is baked to obtain a coated sand shell mold;

[0009] Step 2: adding scrap steel, ferrochrome, nickel plate, ferromolybdenum and ferrovanadium in sequence, and heating and melting to obtain molten steel;

[0010] Step 3: Add calcium silicide and aluminum wire to the molten steel, remove the molten steel from the furnace after deoxidation, and add ferroniobium, ferrocobalt and calcium silicide before removing the molten steel from the furnace;

[0011] Step 4: pour the molten steel in step 3 into a pouring ladle, add calcium silicide and aluminum wire into the ladle, heat the molten steel, deoxidize it, and add ferrotelluride, ferrocerium, aluminum, and calcium silicide into the ladle before tapping;

[0012] Step 5: Pour the molten steel in step 4 into the ladle, remove the slag, let it stand, pour it into the coated sand shell mold, and cool it to form a high-strength high-temperature oxidation-resistant grate bar.

[0013] Furthermore, in step 1, the particle size of the coated sand is 70-140 mesh, the heating temperature is 250-260° C., the curing time is 300-360 s, and the sand-shooting pressure is 0.55-0.65 MPa.

[0014] Furthermore, in step 1, the baking temperature is 120-140° C., and the baking time is 50-60 min.

[0015] Furthermore, in step 1, the tensile strength of the coated sand shell mold at room temperature is 4.0 to 4.5 MPa; the flexural strength at room temperature is 6 to 8 MPa.

[0016] Furthermore, in step 2, the heating melting temperature is 1660-1680°C.

[0017] Furthermore, in step 3, the amount of calcium silicide added accounts for 0.2% of the mass of the molten steel; the amount of aluminum wire used accounts for 0.01% of the mass of the molten steel.

[0018] Furthermore, in step 4, the amount of calcium silicide added accounts for 0.2% of the mass of the molten steel; the amount of aluminum wire used accounts for 0.01% of the mass of the molten steel.

[0019] Furthermore, in step 4, the temperature of the molten steel is raised to 1660-1680°C.

[0020] Furthermore, in step 5, the slag removal is performed 2 to 3 times.

[0021] Furthermore, in step 5, the contents of each element in the grate bars are calculated by weight percentage: 0.2-0.45% carbon, 1.0-2.0% silicon, 0.7-0.9% manganese, 0-0.04% phosphorus, 0-0.03% sulfur, 24-27% chromium, 0.15-0.2% molybdenum, 11-12% nickel, 0.14-0.2% cobalt, 0.15-0.2% vanadium, 0.35-0.45% niobium, 0-0.005% tellurium, 0-0.05% cerium, and the remainder is iron.

[0022] Compared with the prior art, the present invention has the following beneficial effects: the present invention increases the chromium content in the alloy to 24-27%, and at the same time appropriately reduces the carbon content to 0.2-0.5%, thereby avoiding the chromium deficiency phenomenon and preventing the formation of chromium carbide (Cr 3 C 2 ), so that the grain boundaries are depleted in chromium (chromium depletion will occur if the grain boundary layer is less than 17%), and finally the oxidation resistance and high temperature strength of the alloy material are improved. In addition, the present invention reduces the amount of precious metal nickel added by the microalloying method, but at the same time ensures that its performance is equivalent to that of 2520 material with a nickel content of 20%, greatly reducing the material cost, while improving the high temperature strength, high temperature oxidation resistance, and high temperature corrosion resistance of the material. The use effect is much higher than that of conventional high chromium cast iron grates, and the service life can reach 3 to 5 years. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0024] Figure 1 It is a metallographic diagram of the product in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Embodiment 1: A high-strength high-temperature oxidation-resistant grate bar and a preparation method thereof, comprising the following steps:

[0027] Step 1: Prepare coated sand for shell core:

[0028] Take the coated sand, heat it at 250°C, solidify it for 300s, and the sand shooting pressure is 0.6MPa to obtain a coated sand shell mold. Wet the surface of the coated sand shell mold with a water-based coating, and then bake the shell mold at a baking temperature of 140°C and a baking time of 60min to obtain a coated sand shell mold.

[0029] Step 2: Add scrap steel, ferrochrome, nickel plate, ferromolybdenum and ferrovanadium in sequence, raise the temperature to 1660°C, heat and melt to obtain molten steel;

[0030] Step 3: Add 0.2% calcium silicide and 0.01% aluminum wire to the molten steel, deoxidize the molten steel in the furnace, and add ferroniobium, ferrocobalt and calcium silicide 10 minutes before the molten steel is taken out of the furnace;

[0031] Step 4: pour the molten steel in step 3 into a pouring ladle, add 0.2% calcium silicide and 0.01% aluminum wire to the ladle, heat the molten steel to 1680°C, deoxidize, and add ferrotelluride, ferrocerium, aluminum, and calcium silicide to the ladle before tapping;

[0032] Step 5: After the molten steel in step 4 is poured into the ladle, the slag is removed for 3 times, and the slag is allowed to stand for 3 minutes, and then poured into the coated sand shell mold, and cooled and formed to obtain high-strength high-temperature oxidation-resistant grate bars. The content of each element in the grate bars is calculated by weight percentage: 0.23% carbon, 1.26% silicon, 0.77% manganese, 0.023% phosphorus, 0.01% sulfur, 26.47% chromium, 0.2% molybdenum, 11.89% nickel, 0.18% cobalt, 0.19% vanadium, 0.39% niobium, 0.005% tellurium, 0.05% cerium, and the remainder is iron.

[0033] Embodiment 2: A high-strength high-temperature oxidation-resistant grate bar and a preparation method thereof, comprising the following steps:

[0034] Step 1: Prepare coated sand for shell core:

[0035] Take the coated sand, heat it at 260℃, solidify it for 300s, and the sand shooting pressure is 0.6MPa to obtain a coated sand shell mold. Wet the surface of the coated sand shell mold with a water-based coating, and then bake the shell mold at a baking temperature of 130℃ and a baking time of 60min to obtain a coated sand shell mold.

[0036] Step 2: Add scrap steel, ferrochrome, nickel plate, ferromolybdenum and ferrovanadium in sequence, raise the temperature to 1660°C, heat and melt to obtain molten steel;

[0037] Step 3: Add 0.2% calcium silicide and 0.01% aluminum wire to the molten steel, deoxidize the molten steel in the furnace, and add ferroniobium, ferrocobalt and calcium silicide 10 minutes before the molten steel is taken out of the furnace;

[0038] Step 4: pour the molten steel in step 3 into a pouring ladle, add 0.2% calcium silicide and 0.01% aluminum wire to the ladle, heat the molten steel to 1670°C, deoxidize, and add ferrotelluride, ferrocerium, aluminum, and calcium silicide to the ladle before tapping;

[0039] Step 5: After the molten steel in step 4 is poured into a ladle, the slag is removed for 2 times, and the slag is allowed to stand for 3 minutes, and then poured into a coated sand shell mold, and cooled and formed to obtain a high-strength high-temperature oxidation-resistant grate bar; the content of each element in the grate bar is calculated by weight percentage: 0.233% carbon, 1.23% silicon, 0.8% manganese, 0.023% phosphorus, 0.01% sulfur, 26.54% chromium, 0.2% molybdenum, 11.47% nickel, 0.18% cobalt, 0.19% vanadium, 0.39% niobium, 0.005% tellurium, 0.05% cerium, and the remainder is iron.

[0040] Embodiment 3: A high-strength high-temperature oxidation-resistant grate bar and a preparation method thereof, comprising the following steps:

[0041] Step 1: Prepare coated sand for shell core:

[0042] Take the coated sand, heat it at 255°C, solidify it for 300s, and the sand shooting pressure is 0.6MPa to obtain a coated sand shell mold. Wet the surface of the coated sand shell mold with a water-based coating, and then bake the shell mold at a baking temperature of 140°C and a baking time of 60min to obtain a coated sand shell mold.

[0043] Step 2: Add scrap steel, ferrochrome, nickel plate, ferromolybdenum and ferrovanadium in sequence, raise the temperature to 1660°C, heat and melt to obtain molten steel;

[0044] Step 3: Add 0.2% calcium silicide and 0.01% aluminum wire to the molten steel, deoxidize the molten steel in the furnace, and add ferroniobium, ferrocobalt and calcium silicide 10 minutes before the molten steel is taken out of the furnace;

[0045] Step 4: pour the molten steel in step 3 into a pouring ladle, add 0.2% calcium silicide and 0.01% aluminum wire to the ladle, heat the molten steel to 1675°C, deoxidize, and add ferrotelluride, ferrocerium, aluminum, and calcium silicide to the ladle before tapping;

[0046] Step 5: After the molten steel in step 4 is poured into the ladle, the slag is removed for 3 times, and the slag is allowed to stand for 4.5 minutes, and then poured into the coated sand shell mold, and cooled and formed to obtain high-strength high-temperature oxidation-resistant grate bars. The content of each element in the grate bars is calculated by weight percentage: 0.216% carbon, 1.23% silicon, 0.8% manganese, 0.031% phosphorus, 0.01% sulfur, 24.26% chromium, 0.2% molybdenum, 11.69% nickel, 0.18% cobalt, 0.19% vanadium, 0.39% niobium, 0.005% tellurium, 0.05% cerium, and the remainder is iron.

[0047] Embodiment 4: A high-strength high-temperature oxidation-resistant grate bar and a preparation method thereof, comprising the following steps:

[0048] Step 1: Prepare coated sand for shell core:

[0049] Take the coated sand, heat it at 260℃, solidify it for 300s, and the sand shooting pressure is 0.6MPa to obtain a coated sand shell mold. Wet the surface of the coated sand shell mold with a water-based coating, and then bake the shell mold at a baking temperature of 140℃ for 60min to obtain a coated sand shell mold.

[0050] Step 2: Add scrap steel, ferrochrome, nickel, ferromolybdenum and ferrovanadium in sequence, raise the temperature to 1660°C, heat and melt to obtain molten steel;

[0051] Step 3: Add 0.2% calcium silicide and 0.01% aluminum wire to the molten steel, deoxidize the molten steel in the furnace, and add ferroniobium, ferrocobalt and calcium silicide 10 minutes before the molten steel is taken out of the furnace;

[0052] Step 4: pour the molten steel in step 3 into a pouring ladle, add 0.2% calcium silicide and 0.01% aluminum wire to the ladle, heat the molten steel to 1680°C, deoxidize, and add ferrotelluride, ferrocerium, aluminum, and calcium silicide to the ladle before tapping;

[0053] Step 5: After the molten steel in step 4 is poured into the ladle, the slag is removed for 3 times, and the slag is allowed to stand for 3 minutes, and then poured into the coated sand shell mold, and cooled and formed to obtain high-strength high-temperature oxidation-resistant grate bars. The content of each element in the grate bars is calculated by weight percentage: 0.233% carbon, 0.86% silicon, 0.8% manganese, 0.022% phosphorus, 0.01% sulfur, 26.43% chromium, 0.2% molybdenum, 11.66% nickel, 0.18% cobalt, 0.19% vanadium, 0.39% niobium, 0.005% tellurium, 0.05% cerium, and the remainder is iron.

[0054] Comparative Example 1: Commercially available grate bar, item number GX40CrNiSi25-20, nickel content 21%.

[0055] The performance tests were performed on the grate bars in Examples 1 to 4 and Comparative Example 1, wherein the test method was based on GB / T228-2015 room temperature tensile test method for metal materials; the test results are shown in the following table:

[0056]

[0057]

[0058] Conclusion: Through the above mechanical property comparison of the grate bars prepared by the present invention, the performance of the grate bars developed by our company is higher than that of similar foreign products of the same kind; through the chemical composition comparison, the nickel content in the grate bars developed by our company is greatly reduced.

[0059] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0060] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing high-strength high-temperature oxidation-resistant grate bars, Features: The following steps are involved: Step 1: Take the coated sand, heat it, solidify it, and shoot it to obtain a coated sand shell mold, infiltrate the surface of the coated sand shell mold with a water-based coating, and then bake the shell mold to obtain a coated sand shell mold; Step 2: adding scrap steel, ferrochrome, nickel, ferromolybdenum and ferrovanadium in sequence, and heating and melting to obtain molten steel; Step 3: Add calcium silicide and aluminum wire to the molten steel, remove the molten steel from the furnace after deoxidation, and add ferroniobium, ferrocobalt and calcium silicide before removing the molten steel from the furnace; Step 4: pour the molten steel in step 3 into a pouring ladle, add calcium silicide and aluminum wire into the ladle, heat the molten steel, deoxidize it, and add ferrotelluride, ferrocerium, aluminum, and calcium silicide into the ladle before tapping; Step 5: After the molten steel in step 4 is poured into a ladle, the slag is removed, the molten steel is allowed to stand, and the molten steel is poured into a coated sand shell mold, and the molten steel is cooled and formed to obtain a high-strength high-temperature oxidation-resistant grate bar; the content of each element in the grate bar is calculated by weight percentage: 0.2-0.45% carbon, 1.0-2.0% silicon, 0.7-0.9% manganese, 0-0.04% phosphorus, 0-0.03% sulfur, 24-27% chromium, 0.15-0.2% molybdenum, 11-12% nickel, 0.14-0.2% cobalt, 0.15-0.2% vanadium, 0.35-0.45% niobium, 0-0.005% tellurium, 0-0.05% cerium, and the remainder is iron.

2. A method for preparing a high-strength high-temperature oxidation-resistant grate bar according to claim 1, Features: In step 1, the particle size of the coated sand is 70~140 mesh; the heating temperature is 250~260℃; the curing time is 300~360s; and the sand shooting pressure is 0.55~0.65MPa.

3. A method for preparing a high-strength high-temperature oxidation-resistant grate bar according to claim 1, Features: In step 1, the baking temperature is 120-140° C., and the baking time is 50-60 min.

4. A method for preparing a high-strength high-temperature oxidation-resistant grate bar according to claim 1, Features: In step 1, the tensile strength of the coated sand shell mold at room temperature is 4.0~4.5MPa; the flexural strength at room temperature is 6~8MPa.

5. A method for preparing a high-strength high-temperature oxidation-resistant grate bar according to claim 1, Features: In step 2, the heating melting temperature is 1660~1680℃.

6. A method for preparing a high-strength high-temperature oxidation-resistant grate bar according to claim 1, Features: In step 3, the amount of calcium silicide added accounts for 0.2% of the mass of the molten steel; the amount of aluminum wire used accounts for 0.01% of the mass of the molten steel; in step 4, the amount of calcium silicide added accounts for 0.2% of the mass of the molten steel; the amount of aluminum wire used accounts for 0.01% of the mass of the molten steel.

7. A method for preparing a high-strength high-temperature oxidation-resistant grate bar according to claim 1, Features: In step 4, the molten steel is heated to 1660~1680℃.

8. A grate bar prepared by the method for preparing a high-strength high-temperature oxidation-resistant grate bar according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Fluidized bed furnace central drum alloy and production method thereof

    CN101476087A

  • Grate bar material and production method thereof as well as combined pouring unit of sintering machine

    CN103849819A

  • Medium carbon wear-resistant steel used for high temperature working condition and preparation method thereof

    CN104073745A

  • Blade of sorting machine

    CN104120370A

  • Machining technology of high-chromium cast iron pipe

    CN108273966A