A 3D printed wind turbine blade leading edge protective hydrophilic coating and preparation method thereof

The three-layer hydrophilic coating is prepared through 3D printing technology, and the combination of hole structure and specific components is used to solve the leading edge corrosion problem of wind power blades, improve the durability and protective performance of the coating, and extend the service life of the blades.

CN117447903BActive Publication Date: 2024-11-05HUANENG NEW ENERGY (MENGXI) CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311399308.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-25
Publication Date
2024-11-05
Estimated Expiration
2043-10-25

AI Technical Summary

Technical Problem

The existing coating technology is difficult to improve the protective performance of the leading edge of wind power blades by adjusting the coating structure, resulting in serious problems in blade corrosion and damage, affecting power generation efficiency and safety.

Method used

The three-layer hydrophilic coating is prepared by 3D printing technology. The hardness of the bottom layer, the middle layer and the top layer decreases. The middle layer is a hole structure. The principle of hollow shock absorption is used to buffer the impact of rainwater. Component A is composed of polyetheramine, diisocyanate and poly Aspartate resin, component B consists of isocyanate, blocked isocyanate and solvent-based ceramics, and is printed by laser curing.

Benefits of technology

It significantly improves the durability and protective performance of the coating, and can quickly disperse kinetic energy and potential energy when subjected to strong impact, alleviate rainwater erosion, form water film buffered blades, and extend the service life of the blades.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117447903B_ABST
    Figure CN117447903B_ABST
Patent Text Reader

Abstract

The invention discloses a 3D printed hydrophilic coating for protecting the leading edge of a wind turbine blade and a preparation method thereof. The structure of the coating is provided with three layers, namely, a bottom layer, a middle layer and a top layer are provided in sequence from bottom to top, wherein the bottom layer has the largest hardness and serves as a supporting layer of the entire coating, and the middle layer has the smallest hardness and serves as a buffer layer of the entire coating. When raindrops fall, the hole structure can utilize the hollow shock-absorbing principle, and the porous layer forms an air storage chamber for buffering, so that when the coating is subjected to a strong impact, the kinetic energy and gravitational potential energy generated by the impact are converted into elastic potential energy, and the kinetic energy and potential energy are quickly dispersed through the middle porous layer to alleviate the scouring caused by rainwater, thereby showing longer durability than coatings of general structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of coatings, and in particular relates to a 3D printed wind turbine blade leading edge protective hydrophilic coating and a preparation method thereof. Background Art

[0002] Since blades are the only components of wind turbines to capture wind energy, their safe and stable operation is the basis for wind turbines to obtain higher wind energy utilization coefficients and economic benefits. However, blade damage is also a common problem in wind farms. Therefore, how to protect blades from damage for a long time is a key technology in the wind power industry. A large number of studies have shown that blade leading edge corrosion is one of the important causes of blade damage.

[0003] The leading edge of the blade (from the tip to the position of 1 / 3 of the blade length) is in a high-speed operation state for a long time. It is affected by factors such as aerodynamic friction, aging, rain erosion, salt spray, sand erosion and biological erosion. If no protection is taken, corrosion will generally begin to occur after 0.5-2 years of operation. In mild cases, the leading edge will corrode and become pockmarked, which will change the aerodynamic shape of the blade, increase its resistance and affect the power generation efficiency. For every 80% increase in blade resistance, the power generation will decrease by 5%. The power generation can be reduced by up to 20% due to leading edge corrosion. In severe cases, the blade cracks will widen, grow and deepen, and resistance, noise and whistling will occur during the operation of the fan. At the same time, it will greatly increase the damage and breakage of the blades and deepen the damage to the blades after being struck by lightning, posing a threat to the safe operation of the unit.

[0004] Most existing coatings adjust the coating formula based on the coating components so that the coating performance meets the requirements of the blade leading edge, but there are few methods to improve the coating performance from the coating structure setting.

[0005] On the other hand, the most commonly used coating construction method is spraying, which is suitable for preparing protective coatings on various substrates. In addition, reactive extrusion molding and scraping can also be used for spraying construction of polyurea, but it is difficult to obtain coatings with special structures by spraying, extrusion or scraping. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a 3D printed wind turbine blade leading edge protective hydrophilic coating and a preparation method thereof, so as to solve the defect in the prior art of lacking the ability to improve the blade leading edge coating by adjusting the coating structure.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A 3D printed wind turbine blade leading edge protective hydrophilic coating, comprising a bottom layer, a middle layer and a top layer arranged in sequence from the inside to the outside, the bottom layer has a harderness greater than the top layer, the top layer has a harderness greater than the middle layer; the middle layer has a hole structure;

[0009] The coatings are all prepared by 3D printing of coatings; the coatings are composed of component A and component B, and the mass ratio of component A to component B is 1:1 to 2.2:1; component A is composed of polyetheramine, diisocyanate and polyaspartic acid ester resin, component B is composed of solvent-based ceramics and substance C, and substance C is composed of isocyanate and blocked isocyanate;

[0010] The ratio of solvent-based ceramic to substance C is different in the bottom layer, middle layer and top layer.

[0011] A further improvement of the present invention is:

[0012] Preferably, the thickness of the bottom layer is 80-120 μm, the thickness of the middle layer is 100-180 μm, and the thickness of the top layer is 100-130 μm.

[0013] Preferably, the mass ratio of solvent-based ceramics to substance C in the bottom layer is 0.5-0.8:1, in the middle layer is 0.05-0.1:1, and in the top layer is 0.1-0.35:1.

[0014] Preferably, in the middle layer, the size of the holes is 30-120 μm, the spacing between the holes is 40-200 μm, and the holes are interconnected.

[0015] Preferably, in component A, the molar ratio of polyetheramine to diisocyanate is 1:(1-1.3); the mass ratio of polyaspartic acid ester resin to polyetheramine is (3-8):1;

[0016] Preferably, in component A, the polyetheramine is a mixture of any one or more of polyetheramine M230, polyetheramine M1000 or polyetheramine 2000; the diisocyanate is a mixture of any one or more of isophorone diisocyanate, hexamethylene diisocyanate and 4,4'-dicyclohexylmethane diisocyanate;

[0017] In component A, the polyaspartic acid ester resin is a mixture of F420 and F520, and the molar ratio of the polyaspartic acid ester resin F420 to the polyaspartic acid ester resin F520 is 4-5:1.

[0018] Preferably, in substance C, the mass ratio of isocyanate to blocked isocyanate is 1:2 to 1:4.

[0019] Preferably, the mass ratio of -NCO in substance C to -NH in polyaspartic acid ester resin is (0.9-1.2):1.

[0020] Preferably, in component B, the solvent-based ceramic is composed of triethoxysilane, ethoxyphenyl silicone resin, multifunctional filler and potassium hydroxide alkali glue;

[0021] The mass ratio of triethoxysilane, ethoxyphenyl silicone resin and multifunctional filler is 1:1:1.5, and the mass fraction of potassium hydroxide alkali glue in solvent-based ceramics is 0.1-0.2%.

[0022] A method for preparing the above-mentioned 3D printed wind turbine blade leading edge protective hydrophilic coating, placing component A and component B in two 3D printing heads respectively, pressure extrusion printing, laser curing, repeating the component foundation and laser curing until printing is completed.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention discloses a 3D printed wind turbine blade leading edge protective hydrophilic coating, the structure of the coating is provided with three layers, from bottom to top, the bottom layer, the middle layer and the top layer are sequentially provided, wherein the bottom layer has the largest hardness and serves as the supporting layer of the entire coating, the middle layer has the smallest hardness and serves as the buffer layer of the entire coating, when raindrops fall, the hole structure can utilize the hollow shock absorption principle, the porous layer forms an air storage chamber for buffering, so that when the coating is subjected to a strong impact, the kinetic energy and gravitational potential energy generated by the impact are converted into elastic potential energy, and the middle porous layer will react quickly to quickly disperse the kinetic energy and potential energy, alleviate the scouring caused by rainwater, and then show longer durability than the coating of general structure. In the final printing process of the coating, polyetheramine, diisocyanate, and polyaspartic acid ester resin are used as component A, and component B is made of isocyanate, blocked isocyanate and solvent-based ceramics as raw materials. According to the different hardness of the bottom layer, the middle layer and the top layer, the amount of solvent-based ceramics added is different; with the increase of the amount of solvent-based ceramics, the higher the hardness; so that the above-mentioned coating can achieve different functions.

[0025] Furthermore, in the coating, polyetheramine is a hydrophilic monomer, which makes the system have good hydrophilicity, which is conducive to forming a water film on the leading edge of the wind turbine blade, effectively buffering the impact of raindrops on the leading edge of the wind turbine blade. Diisocyanate can extend the chain of the system to increase the molecular weight of the product, thereby increasing the solid content of the polyurea base material and improving the stability of the solution. Furthermore, the -NCO group can react with the -NH group on the polyaspartic acid ester to generate a urea group, thereby reducing the reactivity of the system. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a coating structure diagram of the present invention;

[0027] Figure 2 A cross-sectional view of the middle layer. DETAILED DESCRIPTION

[0028] See also Figure 1, which is a schematic diagram of the structure of a rain erosion prevention coating for the leading edge of a wind turbine blade disclosed by the present invention, including a three-layer structure arranged from the inside to the outside, a bottom layer, a middle layer and a top layer, the middle layer is a porous flexible layer, and the top layer is a relatively flexible hydrophilic polyurea coating; in terms of hardness, the bottom layer>top layer>middle layer; the three coating components are similar, among which the proportion of ceramic substances is different, and the higher the hardness, the higher the ceramic content. The coating is obtained by printing layer by layer by straight pen 3D printing technology. The thickness is 80-120μm for the bottom layer, 100~180μm for the middle layer, and 100~130μm for the top layer.

[0029] See also Figure 2 The holes in the middle layer are arranged in an array or evenly on the middle layer, that is, the distances between adjacent holes are equal. This structure allows the middle layer to be evenly stressed when impacted, and the holes are interconnected.

[0030] The design basis of the above structure is: "water buffering", which refers to the potential lower erosion rate of a wetted surface compared to a dry surface. In the case of conventional coatings on wind turbine blades under natural exposure, a water film originating from an impact drop may not be allowed to form, which will only exist for a very short time, or be very thin due to the wind speed, which forces any residual water to be blown away. However, in the setting of increasing the strong hydrophilicity of the coating, a thin water film is indeed expected to form and exist when continuous water droplets impact. Subsequently, after impacting the water layer, the water droplets break into thousands of small droplets, which are sent in all directions, greatly easing the impact. A water film can be formed when the rate at which the liquid reaches the surface is high enough to balance the losses due to air friction, rotational removal and water evaporation. When it is hit by a water drop, the liquid film deforms so that the pressure on the surface is less than when the surface is dry. However, this effect is only significant when the liquid film thickness is above a certain critical value (not quantified).

[0031] The impact velocity of water droplets plays a decisive role in the erosion of the leading edge of the blade. The droplet erosion rate is proportional to the seventh power of the droplet velocity. Only when the impact velocity of water droplets is greater than the damage threshold will the material surface be eroded, and increasing the impact frequency of water droplets will increase the damage rate and shorten the damage incubation period. The laminated material with structured geometry designed in the present invention can relieve transient stress in the coating press plate, thereby showing longer durability than flat laminated materials.

[0032] Because the middle layer is a porous structure, the hollow shock-absorbing principle can be used, and the porous layer forms an air storage chamber for buffering. When the coating is subjected to a strong impact, the kinetic energy and gravitational potential energy generated by the impact are converted into elastic potential energy, which will react quickly through the middle porous layer to quickly disperse the kinetic energy and potential energy.

[0033] The coating components are designed as a hydrophilic coating formula, including component A and component B during printing, wherein component A is polyetheramine, diisocyanate and polyaspartic acid ester resin; component B is composed of substance C and solvent-based ceramics, and substance C is composed of isocyanate and blocked isocyanate.

[0034] In some embodiments, the diisocyanate is any one or more of isophorone diisocyanate, hexamethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.

[0035] In some embodiments, the polyetheramine is a mixture of any one or more of polyetheramine M230, polyetheramine M1000, or polyetheramine 2000.

[0036] In some embodiments, the polyaspartic acid ester resin is a mixture of F420 and F520, wherein the molar ratio of the polyaspartic acid ester resin F420 to the polyaspartic acid ester resin F520 is 4-5:1.

[0037] In some embodiments, the molar ratio of polyetheramine to diisocyanate is 1:(1-1.3).

[0038] In some embodiments, the mass ratio of the polyaspartic acid ester resin to the polyetheramine is (3-8):1.

[0039] In some embodiments, the mass ratio of -NCO in substance C to that in polyaspartic acid ester resin is calculated as n(-NCO):n(-NH)=(0.9-1.2):1. Adding blocked isocyanate to substance C can slow down the reaction rate of isocyanate and amine, thereby controlling the coagulation speed.

[0040] In some embodiments, the mass ratio of solvent-based ceramic to substance C in different layers is: 0.5-0.8:1 for the bottom layer, 0.05-0.1:1 for the middle layer, and 0.1-0.35:1 for the top layer.

[0041] The mass ratio of isocyanate to blocked isocyanate in substance C is 1:2 to 1:4.

[0042] In some embodiments, the ceramic is composed of four components: (1) a multifunctional silane coupling agent to undergo a sol-gel reaction to form a dense three-dimensional network cross-linked structure; (2) a multifunctional silicone resin that can participate in the sol-gel reaction of the silane coupling agent to increase the strength and toughness of the three-dimensional cross-linked structure; (3) functional fillers and additives including (reinforcement, toughening, thermal conductivity, wear resistance, ablation resistance, etc.) fillers, leveling agents, dispersants, etc. (4) a catalyst, namely potassium hydroxide alkali gel.

[0043] Specifically, the multifunctional silane coupling agent is triethoxysilane, the multifunctional silicone resin is ethoxyphenyl silicone resin, and the functional filler includes nano titanium dioxide, acrylate, organic amine and dimethyl sulfoxide. The mass ratio of triethoxysilane, ethoxyphenyl silicone resin and functional filler is 1:1:1.5, and the mass fraction of the catalyst in the ceramic is 0.1-0.2%.

[0044] Since polyaspartic acid polyurea reacts rapidly with water, deionized water cannot be used as a solvent for the ceramic base material. The present invention selects dimethyl sulfoxide, a polar organic solvent, as a solvent. After adding a catalyst, the sol-gel reaction in the ceramic base material can be promoted to form a dense three-dimensional network cross-linked structure, which can ensure the stability of the coating after compounding.

[0045] The present invention also discloses a 3D printing preparation method of the above-mentioned coating, using the two-component polyurea material for 3D printing; comprising the following process: the A and B components are pumped to the printing cavity for mixing, printed by pressure extrusion, and laser cured, and the operation is repeated until the printing is completed. Wherein, in terms of mass fraction, the extrusion feed ratio of the printer is between 1:1 and 2.2:1. The printing speed of the printer is: 200-1200mm / min. The laser of the printer is a broad-spectrum light source, and the laser curing time is: 15 seconds to 50 seconds. The porous size of the middle layer is: 30-120μm, and the spacing size is 40-200μm.

[0046] The reaction rate of amino group and isocyanate is very fast, which can easily cause nozzle clogging and make 3D printing difficult. The present invention introduces solvent-based ceramic components and blocked isocyanate to adjust the curing rate of amino group and isocyanate and the viscosity of the system to achieve two-component polyurea direct writing 3D printing.

[0047] One embodiment of the present invention discloses a method for preparing a ceramic base material, comprising the following steps:

[0048] Preparation method of component A

[0049] (1) Weigh polyetheramine and polyaspartic acid ester resin according to a set ratio, place them in a four-necked flask for vacuum drying, and the vacuum drying conditions are: 100 to 105° C., -0.04 to -0.07 MPa, and time is 1 to 1.5 h.

[0050] (2) Weigh the diisocyanate according to the above ratio and place it in a constant pressure titration funnel.

[0051] (3) The four-necked flask containing the polyetheramine and the polyaspartic acid ester resin in step (1) is taken out from the vacuum drying oven, nitrogen is introduced into the flask while the stirrer is turned on, and the temperature is lowered to 30-50° C.

[0052] (4) Open the constant pressure titration funnel in step (2) and add diisocyanate to the four-necked flask at a uniform rate for 1 to 1.5 hours.

[0053] (5) After the dripping is completed, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and drip it into the four-necked flask, raise the temperature to 50-70°C, and react at a constant temperature for 2-3 hours.

[0054] (6) Change the constant pressure titration funnel and slowly add dimethyl sulfoxide to the reaction product of step (5) while stirring. The addition time is 0.5 to 1 h, the stirring speed is 1000 to 1300 r / min, and the stirring time is 0.3 to 0.5 h to obtain component A.

[0055] Preparation method of component B

[0056] Based on n(—NCO):n(—NH)=(0.9-1.2):1, the amount of -NCO in substance C is calculated according to the weight of -NH in the polyaspartic acid ester resin in component A, and the two are fully stirred. According to the position of the coating preparation and the ratio of solvent-based ceramic to substance C in different coatings, the amount of solvent-based ceramic added is determined to obtain component B.

[0057] Specifically, the preparation method of solvent-based ceramics includes the following steps:

[0058] (1) 100 parts of octamethylcyclotetrasiloxane are placed in a beaker, and the beaker is placed in an oil bath; 0.2-0.3 parts of potassium hydroxide are slowly added into the beaker through a funnel, and the mixture is heated to 115-120° C. with stirring. After the potassium hydroxide is completely dissolved, the mixture is cooled to room temperature to obtain a transparent potassium hydroxide alkali gel as a catalyst.

[0059] (2) Weigh triethoxysilane, ethoxyphenyl silicone resin and functional filler of the ceramic respectively, the mass ratio of the three in the ceramic is 1:1:1.5, and weigh the catalyst component D in step (1), the mass content of which is 0.1-0.2% of the total mass.

[0060] (3) Place triethoxysilane, dimethyl sulfoxide and the catalyst in a 50°C water bath and stir for 0.5 to 1 hour at a stirring speed of 100 to 180 r / min.

[0061] (4) Adding ethoxyphenyl silicone resin to the reaction product in step (3), stirring at room temperature for 2 to 2.5 hours at a stirring speed of 400 to 560 r / min.

[0062] (5) Add nano-titanium dioxide, acrylic acid and organic amine to the reaction product of step (4), stir at room temperature for 1 to 1.5 hours at a stirring speed of 400 to 500 r / min to obtain a ceramic base material.

[0063] The present invention is further described in detail below in conjunction with specific embodiments:

[0064] Example 1

[0065] Step 1, preparation of component A

[0066] (1) Weigh polyaspartic acid ester resin and polyetheramine in a mass ratio of 5:1 and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 105° C., −0.05 MPa, and time is 1.5 h.

[0067] (2) Weigh diisocyanate according to the mass ratio of polyaspartic acid ester resin to polyetheramine of 1:1 and place it in a constant pressure titration funnel.

[0068] (3) The four-necked flask containing the polyetheramine and the polyaspartic acid ester resin in step (1) was taken out from the vacuum drying oven, nitrogen was introduced into the flask while the stirrer was turned on, and the temperature was lowered to 40°C.

[0069] (4) Open the constant pressure titration funnel in step (2) and uniformly add the diisocyanate in step (2) to the four-necked flask for 1 h.

[0070] (5) After the dripping is completed, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and drip it into the four-necked flask, raise the temperature to 60°C, and react at the constant temperature for 2 hours.

[0071] (6) Change the constant pressure titration funnel and slowly add dimethyl sulfoxide to the reaction product of step (5) and start stirring. The dropping time is 1 hour, the stirring speed is 1200 r / min, and the stirring time is 0.5 hour to obtain component A.

[0072] Step 2, preparation method of component B

[0073] (1) The amount of -CO in substance C is calculated according to the weight of -NH in the polyaspartic acid ester resin in component A, and the ratio of the two is calculated as n(-NCO):n(-NH)=1:1. Further, isocyanate and blocked isocyanate are weighed respectively at a mass ratio of 1:3.

[0074] (2) Preparation of solvent-based ceramics,

[0075] (2.1) Place 100 parts of octamethylcyclotetrasiloxane in a beaker, and place the beaker in an oil bath; slowly add 0.2 parts of potassium hydroxide into the beaker through a funnel, start stirring and heat to 120° C. After the potassium hydroxide is completely dissolved, cool to room temperature to obtain a transparent potassium hydroxide alkali gel as a catalyst.

[0076] (2.2) Weigh triethoxysilane, ethoxyphenyl silicone resin and functional filler of the ceramic respectively, the mass ratio of the three in the ceramic is 1:1:1.5, and weigh the potassium hydroxide alkali gel in step (1), the mass content of which is 0.2% of the total mass.

[0077] (2.3) Place triethoxysilane, dimethyl sulfoxide and the catalyst in a 50°C water bath and stir for 1 h at a stirring speed of 150 r / min.

[0078] (2.4) Add ethoxyphenyl silicone resin to the reaction product in step (2.3), stir at room temperature for 2 hours at a stirring speed of 500 r / min.

[0079] (2.5) Add nano-titanium dioxide, acrylic acid and organic amine to the reaction product of step (2.4), stir at room temperature for 1 hour at a stirring speed of 400 r / min to obtain a ceramic base material.

[0080] Step 3, the isocyanate, blocked isocyanate and ceramic base material weighed in step (1) are used to form different components B according to the coating at different positions, the mass ratio of ceramic to substance C in the bottom layer is 0.6:1, the mass ratio of ceramic to substance C in the middle layer is 0.08:1, and the mass ratio of ceramic to substance C in the top layer is 0.2:1.

[0081] Step 4: Print the bottom layer, middle layer and top layer in sequence, with an extrusion material ratio of 2:1, a printing speed of 1000 mm / min, a laser curing time of 30 s, and the hole size and spacing size of the middle layer are irregularly set.

[0082] Example 2

[0083] Step 1, preparation of component A

[0084] (1) Weigh polyaspartic acid ester resin and polyetheramine in a mass ratio of 3:1 and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 102° C., −0.07 MPa, and time is 1.3 h.

[0085] (2) Weigh diisocyanate according to the mass ratio of polyaspartic acid ester resin to polyetheramine of 1:1.1 and place it in a constant pressure titration funnel.

[0086] (3) The four-necked flask containing the polyetheramine and the polyaspartic acid ester resin in step (1) was taken out from the vacuum drying oven, nitrogen was introduced into the flask while the stirrer was turned on, and the temperature was lowered to 50° C.

[0087] (4) Open the constant pressure titration funnel in step (2) and uniformly add the diisocyanate in step (2) to the four-necked flask for 1 h.

[0088] (5) After the dripping is completed, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and drip it into the four-necked flask, raise the temperature to 50°C, and react at the constant temperature for 2.5 hours.

[0089] (6) Change the constant pressure titration funnel and slowly add dimethyl sulfoxide to the reaction product of step (5) and start stirring. The dropping time is 0.5 h, the stirring speed is 1000 r / min, and the stirring time is 0.3 h to obtain component A.

[0090] Step 2, preparation method of component B

[0091] (2) The amount of -NH in substance C is calculated according to the weight of -NCO in the polyaspartic acid ester resin in component A, and the ratio of the two is calculated as n(-NCO):n(-NH)=1:1.1. Further, isocyanate and blocked isocyanate are weighed respectively at a mass ratio of 1:2.

[0092] (2) Preparation of solvent-based ceramics,

[0093] (2.1) Place 100 parts of octamethylcyclotetrasiloxane in a beaker, and place the beaker in an oil bath; slowly add 0.3 parts of potassium hydroxide into the beaker through a funnel, start stirring and heat to 115° C. After the potassium hydroxide is completely dissolved, cool to room temperature to obtain a transparent potassium hydroxide alkali gel as a catalyst.

[0094] (2.2) Weigh triethoxysilane, ethoxyphenyl silicone resin and functional filler of the ceramic respectively, the mass ratio of the three in the ceramic is 1:1:1.5, and weigh the potassium hydroxide alkali glue in step (1), the mass content of which is 0.1% of the total mass.

[0095] (2.3) Place triethoxysilane, dimethyl sulfoxide and the catalyst in a 50°C water bath and stir for 0.8 h at a stirring speed of 100 r / min.

[0096] (2.4) Add ethoxyphenyl silicone resin to the reaction product in step (2.3), stir at room temperature for 2.5 hours at a stirring speed of 400 r / min.

[0097] (2.5) Add nano-titanium dioxide, acrylic acid and organic amine to the reaction product of step (2.4), stir at room temperature for 1 hour at a stirring speed of 400 r / min to obtain a ceramic base material.

[0098] Step 3, the isocyanate, blocked isocyanate and ceramic base material weighed in step (1) are used to form different components B according to the coating at different positions, the mass ratio of ceramic to substance C in the bottom layer is 0.5:1, the mass ratio of ceramic to substance C in the middle layer is 0.1:1, and the mass ratio of ceramic to substance C in the top layer is 0.1:1.

[0099] Step 4, print the bottom layer, middle layer and top layer in sequence, the extrusion material ratio is 1:1, the printing speed is 1200mm / min, the laser curing time is 50s, the hole size of the middle layer is 30μm, and the interval size is 40μm.

[0100] Example 3

[0101] Step 1, preparation of component A

[0102] (1) Weigh polyaspartic acid ester resin and polyetheramine in a mass ratio of 4:1 and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 101° C., −0.06 MPa, and time is 1.4 h.

[0103] (2) Weigh diisocyanate according to the mass ratio of polyaspartic acid ester resin to polyetheramine of 1:1.3 and place it in a constant pressure titration funnel.

[0104] (3) The four-necked flask containing the polyetheramine and the polyaspartic acid ester resin in step (1) was taken out from the vacuum drying oven, nitrogen was introduced into the flask while the stirrer was turned on, and the temperature was lowered to 38° C.

[0105] (4) Open the constant pressure titration funnel in step (2) and add the diisocyanate in step (2) to the four-necked flask at a uniform rate for 1.2 h.

[0106] (5) After the dripping is completed, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and drip it into the four-necked flask, raise the temperature to 52°C, and react at this constant temperature for 3 hours.

[0107] (6) Change the constant pressure titration funnel and slowly add dimethyl sulfoxide to the reaction product of step (5) and start stirring. The dropping time is 0.8 h, the stirring speed is 1300 r / min, and the stirring time is 0.4 h to obtain component A.

[0108] Step 2, preparation method of component B

[0109] (3) The amount of -NH in substance C is calculated according to the weight of -NCO in the polyaspartic acid ester resin in component A, and the ratio of the two is calculated as n(-NCO):n(-NH)=1.2:1. Further, isocyanate and blocked isocyanate are weighed respectively at a mass ratio of 1:4.

[0110] (2) Preparation of solvent-based ceramics,

[0111] (2.1) Place 100 parts of octamethylcyclotetrasiloxane in a beaker, and place the beaker in an oil bath; slowly add 0.25 parts of potassium hydroxide into the beaker through a funnel, start stirring and heat to 118° C. After the potassium hydroxide is completely dissolved, cool to room temperature to obtain a transparent potassium hydroxide alkali gel as a catalyst.

[0112] (2.2) Weigh triethoxysilane, ethoxyphenyl silicone resin and functional filler of the ceramic respectively, the mass ratio of the three in the ceramic is 1:1:1.5, and weigh the potassium hydroxide alkali glue in step (1), the mass content of which is 0.15% of the total mass.

[0113] (2.3) Place triethoxysilane, dimethyl sulfoxide and the catalyst in a 50°C water bath and stir for 0.5 h at a stirring speed of 180 r / min.

[0114] (2.4) Add ethoxyphenyl silicone resin to the reaction product in step (2.3), stir at room temperature for 2.2 hours at a stirring speed of 560 r / min.

[0115] (2.5) Add nano-titanium dioxide, acrylic acid and organic amine to the reaction product of step (2.4), stir at room temperature for 2.2 hours at a stirring speed of 400 r / min to obtain a ceramic base material.

[0116] Step 3, the isocyanate, blocked isocyanate and ceramic base material weighed in step (1) are used to form different components B according to the coating at different positions, the mass ratio of ceramic to substance C in the bottom layer is 0.8:1, the mass ratio of ceramic to substance C in the middle layer is 0.05:1, and the mass ratio of ceramic to substance C in the top layer is 0.35:1.

[0117] Step 4, print the bottom layer, middle layer and top layer in sequence, the extrusion material ratio is 1.5:1, the printing speed is 500mm / min, the laser curing time is 15s, the hole size of the middle layer is 120μm, and the interval size is 200μm.

[0118] Example 4

[0119] Step 1, preparation of component A

[0120] (1) Weigh polyaspartic acid ester resin and polyetheramine in a mass ratio of 6:1 and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 104° C., −0.05 MPa, and time is 1.2 h.

[0121] (2) Weigh diisocyanate according to the mass ratio of polyaspartic acid ester resin to polyetheramine of 1:1.2 and place it in a constant pressure titration funnel.

[0122] (3) The four-necked flask containing the polyetheramine and the polyaspartic acid ester resin in step (1) was taken out from the vacuum drying oven, nitrogen was introduced into the flask while the stirrer was turned on, and the temperature was lowered to 40°C.

[0123] (4) Open the constant pressure titration funnel in step (2) and uniformly add the diisocyanate in step (2) to the four-necked flask for 1 h.

[0124] (5) After the dripping is completed, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and drip it into the four-necked flask, raise the temperature to 60°C, and react at the constant temperature for 2 hours.

[0125] (6) Change the constant pressure titration funnel and slowly add dimethyl sulfoxide to the reaction product of step (5) and start stirring. The dropping time is 1 hour, the stirring speed is 1200 r / min, and the stirring time is 0.5 hour to obtain component A.

[0126] Step 2, preparation method of component B

[0127] (4) The amount of -NCO in substance C is calculated according to the weight of -NH in the polyaspartic acid ester resin in component A, and the ratio of the two is calculated as n(-NCO):n(-NH)=0.9:1. Furthermore, isocyanate and blocked isocyanate are weighed respectively at a mass ratio of 1:3.

[0128] (2) Preparation of solvent-based ceramics,

[0129] (2.1) Place 100 parts of octamethylcyclotetrasiloxane in a beaker, and place the beaker in an oil bath; slowly add 0.22 parts of potassium hydroxide into the beaker through a funnel, start stirring and heat to 120° C. After the potassium hydroxide is completely dissolved, cool to room temperature to obtain a transparent potassium hydroxide alkali gel as a catalyst.

[0130] (2.2) Weigh triethoxysilane, ethoxyphenyl silicone resin and functional filler of the ceramic respectively, the mass ratio of the three in the ceramic is 1:1:1.5, and weigh the potassium hydroxide alkali gel in step (1), the mass content of which is 0.2% of the total mass.

[0131] (2.3) Place triethoxysilane, dimethyl sulfoxide and the catalyst in a 50°C water bath and stir for 1 h at a stirring speed of 150 r / min.

[0132] (2.4) Add ethoxyphenyl silicone resin to the reaction product in step (2.3), stir at room temperature for 2 hours at a stirring speed of 500 r / min.

[0133] (2.5) Add nano-titanium dioxide, acrylic acid and organic amine to the reaction product of step (2.4), stir at room temperature for 1 hour at a stirring speed of 400 r / min to obtain a ceramic base material.

[0134] Step 3, the isocyanate, blocked isocyanate and ceramic base material weighed in step (1) are used to form different components B according to the coating at different positions, the mass ratio of ceramic to substance C in the bottom layer is 0.7:1, the mass ratio of ceramic to substance C in the middle layer is 0.1:1, and the mass ratio of ceramic to substance C in the top layer is 0.25:1.

[0135] Step 4, print the bottom layer, middle layer and top layer in sequence, the extrusion material ratio is 2.2:1, the printing speed is 1000mm / min, the laser curing time is 30s, the hole size of the middle layer is 50μm, and the interval size is 150μm.

[0136] Example 5

[0137] Step 1, preparation of component A

[0138] (1) Weigh polyaspartic acid ester resin and polyetheramine in a mass ratio of 7:1 and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 105° C., −0.05 MPa, and time is 1.5 h.

[0139] (2) Weigh diisocyanate according to the mass ratio of polyaspartic acid ester resin to polyetheramine of 1:1 and place it in a constant pressure titration funnel.

[0140] (3) The four-necked flask containing the polyetheramine and the polyaspartic acid ester resin in step (1) was taken out from the vacuum drying oven, nitrogen was introduced into the flask while the stirrer was turned on, and the temperature was lowered to 40°C.

[0141] (4) Open the constant pressure titration funnel in step (2) and uniformly add the diisocyanate in step (2) to the four-necked flask for 1 h.

[0142] (5) After the dripping is completed, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and drip it into the four-necked flask, raise the temperature to 60°C, and react at the constant temperature for 2 hours.

[0143] (6) Change the constant pressure titration funnel and slowly add dimethyl sulfoxide to the reaction product of step (5) and start stirring. The dropping time is 1 hour, the stirring speed is 1200 r / min, and the stirring time is 0.5 hour to obtain component A.

[0144] Step 2, preparation method of component B

[0145] (5) The amount of -NCO in substance C is calculated according to the weight of -NH in the polyaspartic acid ester resin in component A, and the ratio of the two is calculated as n(-NCO):n(-NH)=1:1. Furthermore, isocyanate and blocked isocyanate are weighed respectively at a mass ratio of 1:2.

[0146] (2) Preparation of solvent-based ceramics,

[0147] (2.1) Place 100 parts of octamethylcyclotetrasiloxane in a beaker, and place the beaker in an oil bath; slowly add 0.2 parts of potassium hydroxide into the beaker through a funnel, start stirring and heat to 120° C. After the potassium hydroxide is completely dissolved, cool to room temperature to obtain a transparent potassium hydroxide alkali gel as a catalyst.

[0148] (2.2) Weigh triethoxysilane, ethoxyphenyl silicone resin and functional filler of the ceramic respectively, the mass ratio of the three in the ceramic is 1:1:1.5, and weigh the potassium hydroxide alkali gel in step (1), the mass content of which is 0.2% of the total mass.

[0149] (2.3) Place triethoxysilane, dimethyl sulfoxide and the catalyst in a 50°C water bath and stir for 1 h at a stirring speed of 150 r / min.

[0150] (2.4) Add ethoxyphenyl silicone resin to the reaction product in step (2.3), stir at room temperature for 2 hours at a stirring speed of 500 r / min.

[0151] (2.5) Add nano-titanium dioxide, acrylic acid and organic amine to the reaction product of step (2.4), stir at room temperature for 1 hour at a stirring speed of 400 r / min to obtain a ceramic base material.

[0152] Step 3, the isocyanate, blocked isocyanate and ceramic base material weighed in step (1) are used to form different components B according to the coating at different positions, the mass ratio of ceramic to substance C in the bottom layer is 0.6:1, the mass ratio of ceramic to substance C in the middle layer is 0.08:1, and the mass ratio of ceramic to substance C in the top layer is 0.3:1.

[0153] Step 4: Print the bottom layer, middle layer and top layer in sequence, with an extrusion material ratio of 1:1, a printing speed of 800 mm / min, a laser curing time of 20 s, and the hole size and spacing size of the middle layer are irregularly set.

[0154] Example 6

[0155] Step 1, preparation of component A

[0156] (1) Weigh polyaspartic acid ester resin and polyetheramine in a mass ratio of 8:1 and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 105° C., −0.05 MPa, and time is 1.5 h.

[0157] (2) Weigh diisocyanate according to the mass ratio of polyaspartic acid ester resin to polyetheramine of 1:1.1 and place it in a constant pressure titration funnel.

[0158] (3) The four-necked flask containing the polyetheramine and the polyaspartic acid ester resin in step (1) was taken out from the vacuum drying oven, nitrogen was introduced into the flask while the stirrer was turned on, and the temperature was lowered to 40°C.

[0159] (4) Open the constant pressure titration funnel in step (2) and uniformly add the diisocyanate in step (2) to the four-necked flask for 1 h.

[0160] (5) After the dripping is completed, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and drip it into the four-necked flask, raise the temperature to 60°C, and react at the constant temperature for 2 hours.

[0161] (6) Change the constant pressure titration funnel and slowly add dimethyl sulfoxide to the reaction product of step (5) and start stirring. The dropping time is 1 hour, the stirring speed is 1200 r / min, and the stirring time is 0.5 hour to obtain component A.

[0162] Step 2, preparation method of component B

[0163] (6) The amount of -NCO in substance C was calculated according to the weight of -NH in the polyaspartic acid ester resin in component A, and the ratio of the two was calculated as n(-NCO):n(-NH)=1.2:1. Furthermore, isocyanate and blocked isocyanate were weighed respectively at a mass ratio of 1:4.

[0164] (2) Preparation of solvent-based ceramics,

[0165] (2.1) Place 100 parts of octamethylcyclotetrasiloxane in a beaker, and place the beaker in an oil bath; slowly add 0.2 parts of potassium hydroxide into the beaker through a funnel, start stirring and heat to 120° C. After the potassium hydroxide is completely dissolved, cool to room temperature to obtain a transparent potassium hydroxide alkali gel as a catalyst.

[0166] (2.2) Weigh triethoxysilane, ethoxyphenyl silicone resin and functional filler of the ceramic respectively, the mass ratio of the three in the ceramic is 1:1:1.5, and weigh the potassium hydroxide alkali gel in step (1), the mass content of which is 0.2% of the total mass.

[0167] (2.3) Place triethoxysilane, dimethyl sulfoxide and the catalyst in a 50°C water bath and stir for 1 h at a stirring speed of 150 r / min.

[0168] (2.4) Add ethoxyphenyl silicone resin to the reaction product in step (2.3), stir at room temperature for 2 hours at a stirring speed of 500 r / min.

[0169] (2.5) Add nano-titanium dioxide, acrylic acid and organic amine to the reaction product of step (2.4), stir at room temperature for 1 hour at a stirring speed of 400 r / min to obtain a ceramic base material.

[0170] Step 3, the isocyanate, blocked isocyanate and ceramic base material weighed in step (1) are used to form different components B according to the coating at different positions, the mass ratio of ceramic to substance C in the bottom layer is 0.5:1, the mass ratio of ceramic to substance C in the middle layer is 0.09:1, and the mass ratio of ceramic to substance C in the top layer is 0.2:1.

[0171] Step 4: Print the bottom layer, middle layer and top layer in sequence, with an extrusion material ratio of 2:1, a printing speed of 1000 mm / min, a laser curing time of 30 s, and the hole size and spacing size of the middle layer are irregularly set.

[0172] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A 3D printed wind turbine blade leading edge protective hydrophilic coating, characterized in that: It includes a bottom layer, a middle layer and a top layer arranged in sequence from the inside to the outside, the bottom layer has a harderness than the top layer, and the top layer has a harderness than the middle layer; The middle layer is a hole structure; The coatings are all prepared by 3D printing; the coatings are composed of component A and component B, and the mass ratio of component A to component B is 1:1 to 2.2:1; Component A is composed of polyetheramine, diisocyanate and polyaspartic acid ester resin, component B is composed of solvent-based ceramic and substance C, and substance C is composed of isocyanate and blocked isocyanate; The ratio of solvent-based ceramic and substance C is different in the bottom, middle, and top layers; The mass ratio of the solvent-based ceramic to the substance C in the bottom layer is 0.5-0.8:1, the mass ratio of the solvent-based ceramic to the substance C in the middle layer is 0.05-0.1:1, and the mass ratio of the solvent-based ceramic to the substance C in the top layer is 0.1-0.35:1; In component A, the molar ratio of polyetheramine to diisocyanate is 1:(1-1.3); the mass ratio of polyaspartic acid resin to polyetheramine is (3-8):1; In substance C, the mass ratio of isocyanate to blocked isocyanate is 1:2~1:4; The mass ratio of -NCO in substance C to -NH in polyaspartic acid resin is (0.9~1.2):1; In component B, the solvent-based ceramic is composed of triethoxysilane, ethoxyphenyl silicone resin, multifunctional filler and potassium hydroxide alkali glue; The mass ratio of triethoxysilane, ethoxyphenyl silicone resin and multifunctional filler is 1:1:1.5, and the mass fraction of potassium hydroxide alkali glue in solvent-based ceramics is 0.1-0.2%; The thickness of the bottom layer is 80-120 μm, the thickness of the middle layer is 100-180 μm, and the thickness of the top layer is 100-130 μm; In the middle layer, the size of the holes is 30~120μm, the spacing between the holes is 40~200μm, and the holes are interconnected.

2. The 3D printed wind turbine blade leading edge protective hydrophilic coating according to claim 1, characterized in that: In component A, the polyetheramine is a mixture of any one or more of polyetheramine M230, polyetheramine M1000 or polyetheramine 2000; the diisocyanate is a mixture of any one or more of isophorone diisocyanate, hexamethylene diisocyanate and 4,4'-dicyclohexylmethane diisocyanate; In component A, the polyaspartic acid ester resin is a mixture of F420 and F520, and the molar ratio of the polyaspartic acid ester resin F420 to the polyaspartic acid ester resin F520 is 4-5:

1.

3. A method for preparing a 3D printed wind turbine blade leading edge protective hydrophilic coating according to claim 1, characterized in that: Place component A and component B in two 3D printing heads respectively, perform pressure extrusion printing, and use laser curing. Repeat the component base and laser curing until printing is completed.

Citation Information

Patent Citations

  • Film material for thermosetting resin molding and molded product thereof

    CN112238664A

  • Abrasion-resistant coating for front edge of wind power blade and preparation method of abrasion-resistant coating

    CN113522697A

  • Radix asparagi polyurea wind turbine blade gel coat and preparation method thereof

    CN115960525A

  • Method and coating for protecting and repairing an airfoil surface

    US20120156049A1

  • Methods for manufacturing wind turbine blades and leading edge protection surfaces

    US20220250308A1