A rhenium-doped lithium germanium phosphorus-sulfur sulfide solid electrolyte and preparation method thereof

By doping rhenium elements into lithium germanium phosphorus and sulfur solid electrolytes to form Re-S bonds and Li-Re alloys, the low conductivity and instability of lithium germanium phosphorus and sulfur solid electrolytes are solved, and higher electrochemistry is achieved Stability and cycle life improve the safety and performance of all-solid-state lithium-ion batteries.

CN117457973BActive Publication Date: 2024-12-06SHANGHAI FIRM LITHIUM NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311544050.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-17
Publication Date
2024-12-06
Estimated Expiration
2043-11-17

AI Technical Summary

Technical Problem

The existing lithium germanium phosphorus and sulfur solid electrolytes have low ionic conductivity, unstable electrochemical window and poor stability of lithium metal, resulting in insufficient safety and cycle life of all-solid lithium-ion batteries.

Method used

By doping rhenium elements, the formation of Re-S bonds and Li-Re alloys will improve the stability and electrochemical window of the lithium ion channel, enhance the stability to lithium, and prepare the Li10Ge1-3/4yReyP2S12 type rhenium doped lithium germanium Phosphorus sulfide solid electrolyte.

Benefits of technology

It significantly improves lithium ion conductivity and electrochemical stability, can operate in high voltage environments, extends the cycle life and rate performance of the battery, and improves the safety and efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117457973B_ABST
    Figure CN117457973B_ABST
Patent Text Reader

Abstract

The present invention relates to a rhenium-doped lithium germanium phosphorus sulfur type sulfide solid electrolyte and a preparation method thereof. The lithium germanium phosphorus sulfur type sulfide solid electrolyte of the present invention has a chemical formula of Li 10 Ge 1‑3 / 4y Re y P2S 12 , where 0
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium ion batteries, and in particular relates to a rhenium-doped lithium germanium phosphorus-sulfur sulfide solid electrolyte and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have currently occupied the electric vehicle market in my country and are also being used on a large scale in the grid energy storage market. Battery technology is one of the key technologies to solve the current energy problem. In the battery technology of electric vehicles, energy density is the first indicator of power battery performance, while energy storage batteries pay more attention to cost and safety. With the growth of electric vehicle sales, the frequency of safety accidents such as electrolyte leakage, spontaneous combustion and explosion has also increased significantly, and energy storage power stations have also experienced many safety accidents. Safety issues have become a key issue hindering the further application and development of lithium-ion batteries. The main reason for the safety problem is that flammable organic electrolytes are used in lithium-ion batteries, which participate in combustion and release a lot of heat when the battery has a short-circuit thermal runaway. All-solid-state batteries use solid electrolytes for ion conduction. Compared with traditional liquid batteries, they are non-flammable and non-volatile, and the safety of the battery has been greatly improved. Therefore, they have received widespread attention from academia and industry, and are considered to be one of the most promising next-generation lithium-ion battery technologies.

[0003] Solid electrolytes are the core materials of all-solid-state batteries. Most of the current solid electrolytes have low ion conductivity, unstable electrochemical window and various interface problems. These problems make the comprehensive performance of current all-solid-state batteries unable to meet the application requirements, and there are no commercial products that can be launched. (There are some semi-solid commercial products.) Among the inorganic solid electrolytes reported so far, sulfide electrolytes have attracted much attention due to their highest ionic conductivity and good mechanical properties. However, the disadvantage of lithium-sulfur systems such as Li2S and P2S5 is that they are easily hydrolyzed and oxidized, resulting in poor chemical stability. It is difficult to guarantee long-term stability and cyclability, which restricts the application of lithium-sulfur solid electrolytes. Although Li 10 GeP2S 12 The lithium ion conductivity of (LGPS) can reach the level of commercial liquid electrolytes, but its cost is relatively high, and its application in sulfide solid electrolytes needs to be studied. The present invention effectively solves the problem of Li 10 GeP2S 12 Solid electrolytes have low ionic conductivity and poor stability to lithium metal, and can be used as an ideal solid electrolyte material in all-solid-state lithium secondary batteries. Summary of the invention

[0004] The object of the present invention is to provide a rhenium-doped lithium germanium phosphorus sulfur solid electrolyte and a preparation method thereof in view of the problems existing in the prior art. The rhenium doping in the present invention forms Re-S bonds, and the Re-S bonds are more stable than Ge-S bonds. During the cycling process, they can withstand high voltages, improving the electrochemical window and enabling operation in a high-voltage environment to match different high-voltage cathodes. By forming a Li-Re alloy, a stable alloy is formed during the operation of the battery, which can improve the stability towards Li and has a longer cycle life and rate performance in a full battery. This is related to its lower lattice parameter and larger lithium-ion migration channels.

[0005] The object of the present invention can be achieved by the following solutions:

[0006] The present invention provides a rhenium-doped lithium germanium phosphorus sulfur type sulfide solid electrolyte, and the chemical formula of the lithium germanium phosphorus sulfur type sulfide is Li 10 Ge 1-3 / 4y Re y P2S 12 , where 0 < y ≤ 1.

[0007] Preferably, in the lithium germanium phosphorus sulfur type sulfide solid electrolyte, the range of y is preferably 0 < y ≤ 0.2. Excessive doping amount will also reduce the performance of the electrolyte.

[0008] The present invention also provides a preparation method of the rhenium-doped lithium germanium phosphorus sulfur type sulfide solid electrolyte, including the following steps:

[0009] Step 1: According to the general formula: Li 10 Ge 1-3 / 4y Re y P2S 12 , weigh stoichiometric ratios of Li2S, GeS2, Re2S3, and P2S5;

[0010] Step 2: Grind and mix the raw materials of Li2S, GeS2, Re2S3, and P2S5, and then ball mill to obtain a mixed powder;

[0011] Step 3: Press the mixed powder into tablets, encapsulate after vacuum pumping, and calcine for solid-phase reaction to obtain the lithium germanium phosphorus sulfur type sulfide solid electrolyte.

[0012] Preferably, steps 1, 2, and 3 are all carried out in an argon atmosphere, and the water content of argon is less than 1 ppm, and the oxygen content is less than 1 ppm.

[0013] Preferably, in step 2, the rotation speed of the ball milling is 300 - 600 rpm, preferably 500 - 600 rpm, and the time is 5 - 30 hours. Too low rotation speed of the ball milling leads to poor mixing effect of the raw materials and affects the performance of the electrolyte.

[0014] Preferably, in step 3, the mixed raw material is pressed into a sheet shape so that the components in the mixed raw material are in closer contact and react more fully.

[0015] Preferably, in step 3, the calcination temperature is 500-650° C. and the calcination time is 5-48 hours.

[0016] The present invention also provides an application of the lithium germanium phosphorus-sulfur sulfide solid electrolyte in the preparation of an all-solid-state secondary battery.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] (1) In order to solve the problem that the ion conductivity of the existing lithium-germanium-phosphorus-sulfur solid electrolyte is too low, the present invention uses Re doping to replace Ge with a small atomic radius, thereby expanding the lithium ion channel, improving the ion conductivity, and improving the lithium ion conductivity;

[0019] (2) In order to solve the problem that the electrochemical window of existing lithium germanium phosphorus sulfur solid electrolytes is too narrow, the electrochemical stability of the electrolyte is increased by rhenium doping to form Re-S bonds. Re-S bonds are more stable than Ge-S bonds and can withstand high voltages during the cycle process, thus increasing the electrochemical window (the electrochemical window of LGPS is 1.71-2.14V, and the electrochemical window of rhenium-doped electrolytes is 1V-3.7V). It can operate in a high voltage environment and match different high-voltage positive electrodes;

[0020] (3) In order to solve the problem that the existing lithium-germanium-phosphorus-sulfur solid electrolyte is unstable to the metal Li negative electrode, by forming a Li-Re alloy, a stable alloy is formed during the battery operation, which can improve the stability to Li and have a longer cycle life and rate performance in the full battery;

[0021] (4) Using Re-modified LGPS to match the Li negative electrode can achieve a higher first efficiency of 85%; achieve a higher rate performance up to a cycle rate of 1C; and achieve a capacity retention rate of 90% after 100 cycles at a rate of 0.5C. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0023] Figure 1 The EIS impedance diagrams of the solid electrolytes prepared in the examples and comparative examples;

[0024] Figure 2 The XRD pattern of the solid electrolyte prepared in Example 1;

[0025] Figure 3This is a charge and discharge cycle diagram of a full battery of the material prepared in Example 1 at 1C for 500 cycles. DETAILED DESCRIPTION

[0026] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following examples are implemented on the premise of the technical solution of the present invention, provide detailed implementation methods and specific operation processes, and will help those skilled in the art to further understand the present invention. It should be pointed out that the protection scope of the present invention is not limited to the following embodiments, and several adjustments and improvements made under the premise of the concept of the present invention all belong to the protection scope of the present invention.

[0027] Example 1

[0028] This embodiment provides a method for preparing a 5% rhenium-doped lithium-germanium-phosphorus-sulfur solid electrolyte, comprising the following steps:

[0029] Step 1: Grind and mix Li2S, GeS2, Re2S3 and P2S5 in a molar ratio of 5:0.9625:0.025:1 under an argon atmosphere to obtain a mixed powder.

[0030] Step 2, sealing the mixed powder in a ball milling jar under an argon atmosphere; using a ball mill to ball mill the mixed powder; the speed of the ball mill is 550 rpm, and the ball milling time is 15 hours;

[0031] Step 3, pressing the ball-milled mixed powder into a sheet, placing it into a sealed container, and packaging it after vacuuming; wherein the sheet thickness is 10 mm;

[0032] Step 4, heating and calcining the sample packaged in a sealed container to 650° C., and performing a solid phase reaction for 5 hours;

[0033] Step 5: After the reaction is completed, the mixture is naturally cooled to room temperature to obtain a composition of Li 10 Ge 0.9625 Re 0.05 P2S 12 Doped lithium germanium phosphorus sulfur solid electrolyte material.

[0034] The EIS impedance diagram of the solid electrolyte prepared in Example 1 is as follows: Figure 1 As shown, the XRD spectrum is Figure 2 shown.

[0035] Example 2

[0036] This embodiment provides a method for preparing a 5% rhenium-doped lithium-germanium-phosphorus-sulfur solid electrolyte, comprising the following steps:

[0037] Step 1, grinding and mixing Li2S, GeS2, Re2S3, and P2S5 in a molar ratio of 5:0.9625:0.025:1 under an argon atmosphere to obtain a mixed powder;

[0038] Step 2, sealing the mixed powder in a ball milling jar under an argon atmosphere; using a ball mill to ball mill the mixed powder; the speed of the ball mill is 500 rpm, and the ball milling time is 5 hours; the water content of the argon atmosphere is less than 1 ppm, and the oxygen content is less than 1 ppm;

[0039] Step 3, pressing the ball-milled mixed powder into a sheet, placing it into a sealed container, and packaging it after vacuuming; wherein the sheet thickness is 10 mm;

[0040] Step 4, heating and calcining the sample packaged in a sealed container to 500°C for solid phase reaction for 48 hours;

[0041] Step 5: After the reaction is completed, the mixture is naturally cooled to room temperature to obtain a composition of Li 10 Ge 0.9625 Re 0.05 P2S 12 Doped lithium germanium phosphorus sulfur solid electrolyte material.

[0042] Example 3

[0043] This embodiment provides a method for preparing a 10% rhenium-doped lithium-germanium-phosphorus-sulfur solid electrolyte, comprising the following steps:

[0044] Step 1: Grind and mix Li2S, GeS2, Re2S3 and P2S5 in a molar ratio of 5:0.925:0.05:1 under an argon atmosphere to obtain a mixed powder. Seal the mixture in a ball mill;

[0045] Step 2, sealing the mixed powder in a ball mill jar; using a ball mill to ball mill the mixed powder; the speed of the ball mill is 550 rpm, and the ball milling time is 15 hours;

[0046] Step 3, pressing the ball-milled mixed powder into a sheet, placing it into a sealed container, and packaging it after vacuuming; wherein the sheet thickness is 10 mm;

[0047] Step 4, heating to 500°C and performing solid phase reaction for 48 hours;

[0048] Step 5: After the reaction is completed, the mixture is naturally cooled to room temperature to obtain a composition of Li 10 Ge 0.925 Re 0.1 P2S 12 Doped lithium germanium phosphorus sulfur solid electrolyte material.

[0049] Example 4

[0050] This embodiment provides a method for preparing a 10% rhenium-doped lithium-germanium-phosphorus-sulfur solid electrolyte, comprising the following steps:

[0051] Step 1: Grind and mix Li2S, GeS2, Re2S3 and P2S5 in a molar ratio of 5:0.925:0.05:1 under an argon atmosphere to obtain a mixed powder. Seal the mixture in a ball mill;

[0052] Step 2, sealing the mixed powder in a ball milling jar under an argon atmosphere; using a ball mill to mill the mixed powder; the speed of the ball mill is 300 rpm, and the ball milling time is 30 hours; the water content of the argon atmosphere is less than 1 ppm, and the oxygen content is less than 1 ppm;

[0053] Step 3, pressing the ball-milled mixed powder into a sheet, placing it into a sealed container, and packaging it after vacuuming; wherein the sheet thickness is 10 mm;

[0054] Step 4, heating and calcining the sample packaged in a sealed container to 650°C for solid phase reaction for 5 hours;

[0055] Step 5: After the reaction is completed, the mixture is naturally cooled to room temperature to obtain a composition of Li 9.8 Ge 0.925 Re 0.1 P2S 12 Molybdenum-doped lithium germanium phosphorus sulfur solid electrolyte material. 10 Ge 0.925 Re 0.1 P2S 12 The doped lithium germanium phosphorus sulfur solid electrolyte is ball milled to produce powders of different particle sizes.

[0056] Comparative Example 1

[0057] This comparative example provides a lithium germanium phosphorus sulfur type sulfide solid electrolyte, the chemical formula is Li 10 GeP2S 12 , using corresponding raw materials, the preparation method is basically the same as that in Example 1.

[0058] Comparative Example 2

[0059] This comparative example provides a molybdenum-doped lithium germanium phosphorus sulfur sulfide solid electrolyte, the raw materials are Li2S, GeS2, MoS3, P2S5, the molar ratio is 5:0.925:0.05:1, and the chemical formula is Li 10 Ge 0.925 Mo 0.05 P2S 12 , using corresponding raw materials, the preparation method is basically the same as that in Example 1.

[0060] Comparative Example 3

[0061] This comparative example provides a bismuth-doped lithium germanium phosphorus-sulfur sulfide solid electrolyte, the raw materials are Li2S, CeS2, Bi2S3, P2S5, the molar ratio is 5:0.9625:0.025:1, and the chemical formula is Li 10 Ge 0.9625 Re 0.05 P2S 12 , using corresponding raw materials, the preparation method is basically the same as that in Example 1.

[0062] Comparative Example 4

[0063] This comparative example provides a lanthanum-doped lithium germanium phosphorus sulfur sulfide solid electrolyte, the raw materials are Li2S, GeS2, LaS3, P2S5, the molar ratio is 5:0.925:0.05:1:1, and the chemical formula is Li 10 Ge 0.925 La 0.05 P2S 12 , using corresponding raw materials, the preparation method is basically the same as that in Example 1.

[0064] Performance Verification

[0065] The products obtained in the above-mentioned Examples 1-4 and Comparative Examples 1-5 were assembled: in an inert gas glove box with a water and oxygen content of ≤0.01ppm, the prepared electrolyte was assembled into a battery, with NCM811 for the positive electrode and LiIn alloy for the negative electrode, specifically: 100mg of the prepared rhenium-doped lithium germanium phosphorus sulfur type sulfide solid electrolyte powder was placed in a tablet pressing mold and pressed into a solid electrolyte sheet, then 10mg of NCM811 positive electrode sheet was placed on one side of the solid electrolyte, and pressed at 300Mpa, and finally a LiIn sheet was attached to the other side of the solid electrolyte to press into a full solid-state battery. The cycle stability of the obtained sulfide solid-state battery was tested at room temperature.

[0066] Test conductivity: Use a solid-state battery mold to assemble the battery, then place the mold in a constant temperature box at 25 degrees for charge and discharge testing. First, activate it at 0.1C and then use 1C for a long cycle test.

[0067] 100 mg of the lithium germanium phosphorus sulfur sulfide solid electrolyte powders prepared in Examples 1-4 and Comparative Examples 1-5 were placed in a tableting mold, pressed into solid electrolyte sheets, and tested for conductivity. It can be seen that Example 1 has the lowest impedance and the highest conductivity.

[0068] The sulfide solid-state battery prepared in the embodiment and the comparative example was charged and discharged at 0.1c to test its initial efficiency, and the capacity retention rate was tested after 500 cycles. The full battery of the material prepared in Example 1 was charged and discharged at 1c for 500 cycles. Figure 3As shown, the EIS impedance diagrams of the solid electrolytes of each embodiment and comparative example are as follows Figure 1 As shown, the results are shown in Table 1: According to Table 1, when the doping amount is 5%, the speed of the ball mill is 550 rpm, and the ball milling time is 15 hours, a higher first effect and capacity retention can be achieved, thereby improving the rate performance of the lithium-ion battery.

[0069]

[0070] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A rhenium-doped lithium germanium phosphorus-sulfur sulfide solid electrolyte, It is characterized in that The chemical formula of the lithium germanium phosphorus sulfur sulfide is Li 10 Ge 1-3 / 4y Re y P 2 S 12 , where 0 <y≤0.2。 2. A method for preparing the rhenium-doped lithium germanium phosphorus-sulfur sulfide solid electrolyte as claimed in claim 1, It is characterized in that The following steps are involved: Step 1, according to the general formula: Li 10 Ge 1-3 / 4y Re y P 2 S 12 , weigh the stoichiometric ratio of Li 2 S, GeS 2 、Re 2 S 3 , P 2 S 5 ; Step 2: Li 2 S, GeS 2 、Re 2 S 3 , P 2 S 5 The raw materials are ground and mixed, and then ball-milled to obtain a mixed powder; Step 3: Press the mixed powder into tablets, evacuate the tablets, package them, and calcine them for solid phase reaction to obtain the lithium germanium phosphorus sulfur type sulfide solid electrolyte.

3. The preparation method according to claim 2, It is characterized in that Step 1, step 2 and step 3 are all carried out under an argon atmosphere, and the water content and oxygen content of the argon are less than 1 ppm and less than 1 ppm, respectively.

4. The preparation method according to claim 2, It is characterized in that In step 2, the ball milling speed is 300-600 rpm, and the time is 5-30 hours.

5. The preparation method according to claim 2, It is characterized in that In step 3, the calcination temperature is 500-650° C. and the calcination time is 5-48 hours.

6. Use of the lithium germanium phosphorus sulfur type sulfide solid electrolyte as claimed in claim 1 or the lithium germanium phosphorus sulfur type sulfide solid electrolyte obtained by any preparation method of claims 2 to 5 in the preparation of an all-solid-state secondary battery.

Citation Information

Patent Citations

  • Lithium secondary battery additive, preparation method thereof, and application thereof

    CN110137561A

  • Molybdenum-doped lithium germanium phosphorus sulfur solid electrolyte material and preparation method thereof

    CN114824458A