Preparation method of polyimide fluorescent nanomaterial

The preparation of polyimide nanomaterials by solvent method solves the problems of high production cost and low efficiency in the existing technology, achieves low-cost and efficient preparation, and has application prospects in the fields of new phosphors, sensing and biological imaging.

CN117487160BActive Publication Date: 2024-10-29SUMII TECH (SHENZHEN) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311268424.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-28
Publication Date
2024-10-29
Estimated Expiration
2043-09-28

AI Technical Summary

Technical Problem

The production cost of preparing polyimide nanomaterials in the existing technology is high, the preparation efficiency is low, and the process is complex.

Method used

Using the solvent method, a mixed solution was prepared from 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 2,6-bis(amino-1H-benzo[d]imidazole)pyridine and m-cresol, and then diluted and Dimethylacetamide and industrial alcohol are added dropwise, and polyimide nanomaterials are obtained through dialysis and freeze-drying, and rare earth complexes are introduced to obtain fluorescent materials.

Benefits of technology

The low-cost and efficient preparation of polyimide nanomaterials has been achieved, and has application prospects in the fields of new phosphors, sensing and biological imaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117487160B_ABST
    Figure CN117487160B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a polyimide fluorescent nanomaterial, which specifically comprises the following steps: step 1, using 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride, 2,6-di(amino-1H-benzo[d]imidazole)pyridine, and meta-cresol to prepare a mixed solution; step 2, using dimethylacetamide to dilute the mixed solution prepared in step 1; step 3, dropping industrial alcohol into the diluted solution in step 2 and stirring evenly to obtain a polyimide nanofiber dispersion; step 4, dialyzing the polyimide nanofiber dispersion prepared in step 3, and finally freeze-drying to obtain a polyimide nanomaterial. The polyimide nanomaterial prepared by the method has low cost and simple process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a method for preparing a polyimide fluorescent nano material. Background Art

[0002] Polyimide is widely used in aviation, aerospace, semiconductors, adhesives, coatings and other fields due to its stable structure and good heat resistance. However, the preparation of polyimide nanomaterials is mainly done by electrospinning, which not only has high production costs, but also has a complex preparation process, resulting in reduced preparation efficiency. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a polyimide fluorescent nanomaterial. The polyimide nanomaterial prepared by the method has low cost and high preparation efficiency.

[0004] The technical solution adopted by the present invention is a method for preparing a polyimide fluorescent nanomaterial, which specifically comprises the following steps:

[0005] Step 1, preparing a mixed solution using 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride, 2,6-di(amino-1H-benzo[d]imidazole)pyridine and m-cresol;

[0006] Step 2, diluting the mixed solution prepared in step 1 with dimethylacetamide;

[0007] Step 3, adding industrial alcohol to the diluted solution in step 2 and stirring evenly to obtain a polyimide nanofiber dispersion;

[0008] Step 4, dialyzing the polyimide nanofiber dispersion prepared in step 3, and finally freeze-drying to obtain the polyimide nanomaterial.

[0009] The present invention is also characterized in that:

[0010] The specific process of step 1 is:

[0011] Add 2.24 g of 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride, 3.41 g-6.82 g of 2,6-bis(amino-1H-benzo[d]imidazole)pyridine and 10 mL-20 mL of m-cresol into a reaction bottle, purge with nitrogen for 10 min-30 min to exclude air, then raise the temperature to 100°C-110°C and stir for 10 min-25 min to dissolve all 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride and 2,6-bis(amino-1H-benzo[d]imidazole)pyridine, then add 5 mL-10 mL of m-cresol solution dropwise, raise the temperature to 120°C-140°C and maintain for 0.5 h-1 h, then raise the temperature to 210°C-240°C and react for 8 hours. After the reaction, lower the reaction solution to room temperature to obtain the product.

[0012] The amount of dimethylacetamide used in step 2 is 50mL-100mL.

[0013] In step 3, the amount of industrial alcohol added is 1L to 2L, and the addition time is 1h to 2h.

[0014] The synthetic route of imide nanomaterials is:

[0015]

[0016] The optical modification process of polyimide nanomaterials is as follows: take 0.5g-1g of polyimide nanomaterials, disperse it in 50mL-100mL of a mixed solution of dimethylacetamide and industrial ethanol, add 0.1g-0.2g of NaH and stir evenly, add 0.1g-0.2g of hexafluoroacetylacetone and 0.13g-0.26g of EuCl3.

[0017] The beneficial effect of the present invention is that the present invention can quickly prepare polyimide nanomaterials by using a solvent method. And further introduce a rare earth complex to obtain a polyimide nanomaterial with rare earth characteristic luminescence. The present invention abandons the traditional electrostatic spinning method, and the polyimide nanofluorescence developed has application prospects in the fields of new fluorescent powders, sensors, biological imaging, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a comparison chart of the particle sizes of the polyimide nanomaterial prepared in Example 1 of the method for preparing the polyimide fluorescent nanomaterial of the present invention and the materials prepared in Comparative Examples 1 and 2.

[0019] Figure 2 This is a comparison chart of the luminescence spectrum intensity of the polyimide nanomaterial prepared in Example 1 of the method for preparing the polyimide fluorescent nanomaterial of the present invention and the materials prepared in Comparative Examples 3 and 4. DETAILED DESCRIPTION

[0020] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0021] The preparation method of the polyimide fluorescent nanomaterial of the present invention specifically comprises the following steps:

[0022] 1) Synthesis of polyimide nanomaterials

[0023] 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride (2.24g) and 2,6-di(amino-1H-benzo[d]imidazole)pyridine (3.41g-6.82g) and m-cresol (10mL-20mL) were added to a 100mL reaction bottle, nitrogen was purged for 10min-30min to remove air, and then the temperature was raised to 100℃-110℃ and stirred for 10min-25min to dissolve the above anhydride and diamine raw materials, and then 5mL-10mL of m-cresol solution (containing 0.1-0.2g of isoquinoline, 10min-20min dropwise addition) was gradually added, and the temperature was raised to 120℃-140℃ and maintained for 0.5h-1h, and then the temperature was raised to 210℃-240℃ and reacted for 8h. After the reaction was completed, the reaction solution was cooled to room temperature, and 50mL-100mL of dimethylacetamide was added to dilute the reaction solution to reduce the viscosity of the reaction solution. Finally, the diluted reaction solution was slowly added to 1L-2L of industrial alcohol (addition time 1h-2h) and rapidly stirred at 1200r / min to obtain a polyimide nanofiber dispersion, which was further dialyzed three times using a 7000Da dialysis bag to remove the high boiling point solvent, and finally freeze-dried to obtain a polyimide nanomaterial. The following is the synthesis route of polyimide polymer:

[0024]

[0025] The value of n is related to the molecular weight.

[0026] 2) Optical modification of polyimide nanomaterials

[0027] Take 0.5g-1g of polyimide nanomaterials, disperse them in 50mL-100mL of a mixed solution of dimethylacetamide and industrial ethanol (v:v=1:1), add 0.1-0.2g of NaH and stir at room temperature for 10min. Further add hexafluoroacetylacetone (0.1-0.2g) and EuCl3 (0.13-0.26g).

[0028] Example 1

[0029] 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride (2.24g) and 2,6-di(amino-1H-benzo[d]imidazole)pyridine (3.41g) and m-cresol (10mL) were added to a 100mL reaction bottle, nitrogen was purged for 10min to exclude air, and then the temperature was raised to 100°C and stirred for 10min to dissolve the above anhydride and diamine raw materials, followed by gradual dropwise addition of 5mL of m-cresol solution (containing 0.1g of isoquinoline, added over 10min), and the temperature was raised to 120°C for 0.5 hours, and then raised to 210°C for 8 hours. After the reaction was completed, the reaction solution was cooled to room temperature, and 50mL of dimethylacetamide was added to dilute the reaction solution to reduce the viscosity of the reaction solution. Finally, the diluted reaction solution was slowly added dropwise to 1L of industrial alcohol (addition time 1h) and rapidly stirred at 1200r / min to obtain a polyimide nanofiber dispersion, which was further dialyzed three times using a 7000Da dialysis bag to remove the high boiling point solvent. Finally, the polyimide nanomaterial was freeze-dried.

[0030] Comparative Example 1 (Industrial alcohol was precipitated and replaced with dimethylacetamide, but no nanomaterial was obtained)

[0031] 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride (2.24g) and 2,6-di(amino-1H-benzo[d]imidazole)pyridine (3.41g) and m-cresol (10ml) were added to a 100mL reaction bottle, nitrogen was purged for 10min to exclude air, and then the temperature was raised to 100°C and stirred for 10min to dissolve the above anhydride and diamine raw materials, followed by gradual dropwise addition of 5ml of m-cresol solution (containing 0.1g of isoquinoline, added over 10min), and the temperature was raised to 120°C for 0.5 hours, and then raised to 210°C for 8 hours. After the reaction was completed, the reaction solution was cooled to room temperature, and 50ml of dimethylacetamide was added to dilute the reaction solution to reduce the viscosity of the reaction solution. Finally, the diluted reaction solution was slowly added dropwise to 1L of dimethylacetamide (addition time 1h) and rapidly stirred at 1200r / min to obtain a polyimide nanofiber dispersion, which was further dialyzed three times using a 7000Da dialysis bag to remove the high boiling point solvent. Finally, polyimide powder particles were obtained by freeze drying.

[0032] Comparative Example 2 (removing industrial alcohol sedimentation and not obtaining nanomaterials)

[0033] 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride (2.24g) and 2,6-di(amino-1H-benzo[d]imidazole)pyridine (3.41g) and m-cresol (10ml) were added to a 100mL reaction bottle, nitrogen was purged for 10min to remove air, and then the temperature was raised to 100℃ and stirred for 10min to dissolve all the above anhydride and diamine raw materials. Then 5ml of m-cresol solution (containing 0.1g of isoquinoline, 10min dropwise addition) was gradually added, and the temperature was raised to 120℃ for 0.5 hours, and then the temperature was raised to 210℃ for 8 hours. After the reaction was completed, the reaction solution was cooled to room temperature, and 50ml of dimethylacetamide was added to dilute the reaction solution to reduce the viscosity of the reaction solution. Further, a 7000Da dialysis bag was used for 3 times to remove the high boiling point solvent. Finally, the polyimide powder granular material was obtained by freeze drying.

[0034] from Figure 1 In Example 1, after industrial alcohol precipitation, a nano material with an average hydraulic radius of about 80nm can be obtained, while the hydraulic radius in Comparative Examples 1 and 2 is micrometer-level, and its size is 1.6um and 2.3um respectively. The reason is that the polymer chain is in a stretched state in the dimethylacetamide solution, and after entering the industrial alcohol solvent, the molecular chain curls to form a nano material in Example 1. On the contrary, the polymer in Comparative Examples 1 and 2 is always in a stretched state, and can be frozen later, and the molecular chains are easy to aggregate and crystallize, and the size particle size is larger.

[0035] Comparative Example 3 (NaH was replaced by NaOH, and the luminescence performance was weaker)

[0036] 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride (2.24g) and 2,6-di(amino-1H-benzo[d]imidazole)pyridine (3.41g) and m-cresol (10mL) were added to a 100mL reaction bottle, nitrogen was purged for 10min to exclude air, and then the temperature was raised to 100°C and stirred for 10min to dissolve the above anhydride and diamine raw materials, followed by gradual dropwise addition of 5mL of m-cresol solution (containing 0.1g of isoquinoline, added over 10min), and the temperature was raised to 120°C for 0.5 hours, and then raised to 210°C for 8 hours. After the reaction was completed, the reaction solution was cooled to room temperature, and 50ml of dimethylacetamide was added to dilute the reaction solution to reduce the viscosity of the reaction solution. Finally, the diluted reaction solution was slowly added dropwise to 1L of industrial alcohol (addition time 1h) and rapidly stirred at 1200r / min to obtain a polyimide nanofiber dispersion, which was further dialyzed three times using a 7000Da dialysis bag to remove the high boiling point solvent. Finally, the polyimide nanomaterial was freeze-dried.

[0037] Take 0.5g of polyimide nanomaterial, disperse it in 50-100mL of a mixed solution of dimethylacetamide and industrial ethanol (v:v=1:1), add 0.1g of NaOH and stir at room temperature for 10min. Further add hexafluoroacetylacetone (0.1g) and EuCl3 (0.13g).

[0038] Comparative Example 4 (NaH removed, weak luminescence performance)

[0039] 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride (2.24g) and 2,6-di(amino-1H-benzo[d]imidazole)pyridine (3.41g) and m-cresol (10mL) were added to a 100mL reaction bottle, nitrogen was purged for 10min to exclude air, and then the temperature was raised to 100°C and stirred for 10min to dissolve the above anhydride and diamine raw materials, followed by gradual dropwise addition of 5mL of m-cresol solution (containing 0.1g of isoquinoline, added over 10min), and the temperature was raised to 120°C for 0.5 hours, and then raised to 210°C for 8 hours. After the reaction was completed, the reaction solution was cooled to room temperature, and 50mL of dimethylacetamide was added to dilute the reaction solution to reduce the viscosity of the reaction solution. Finally, the diluted reaction solution was slowly added dropwise to 1L of industrial alcohol (addition time 1h) and rapidly stirred at 1200r / min to obtain a polyimide nanofiber dispersion, which was further dialyzed three times using a 7000Da dialysis bag to remove the high boiling point solvent. Finally, the polyimide nanomaterial was freeze-dried.

[0040] 0.5 g of polyimide nanomaterial was dispersed in 50 mL of a mixed solution of dimethylacetamide and industrial ethanol (v:v=1:1), and 0.1 g of NaOH was added and stirred at room temperature for 10 min. Hexafluoroacetylacetone (0.1 g) and EuCl3 (0.13 g) were further added.

[0041] from Figure 2 It can be seen that the luminescence spectrum intensity in Example 1 is the strongest, and the main reason is that NaH can well remove the NH bond on the imidazole ring of the polyimide polymer chain, which promotes the coordination of Eu3+ and polyimide nanomaterials and the formation of anionic and cationic forces. Secondly, the removal of NH reduces the fluorescence quenching effect of the group. On the contrary, the luminescence of Example 4 is the weakest, because hexafluoroacetylacetone reacts with Eu3+ ions to release H+, and there is no acid binding agent; while the luminescence intensity of Example 3 is strong, although NaOH cannot remove the NH bond, it can be used as an acid binding agent to promote the coordination reaction of Eu3+ and hexafluoroacetylacetone.

[0042] Example 2

[0043] 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride (2.24g) and 2,6-di(amino-1H-benzo[d]imidazole)pyridine (5.5gg) and m-cresol (15mL) were added to a 100mL reaction bottle, nitrogen was purged for 20min to exclude air, and then the temperature was raised to 105°C and stirred for 15min to dissolve the above anhydride and diamine raw materials, followed by gradual dropwise addition of 8mL of m-cresol solution (containing 0.15g of isoquinoline, 15min dropwise addition), and the temperature was raised to 130°C for 0.8 hours, and then raised to 220°C for 8 hours. After the reaction was completed, the reaction solution was cooled to room temperature, and 80mL of dimethylacetamide was added to dilute the reaction solution to reduce the viscosity of the reaction solution. Finally, the diluted reaction solution was slowly added to 1.5L of industrial alcohol (addition time 1.5h) and rapidly stirred at 1200r / min to obtain a polyimide nanofiber dispersion, which was further dialyzed three times using a 7000Da dialysis bag to remove the high boiling point solvent. Finally, the polyimide nanomaterial was freeze-dried.

[0044] Example 3

[0045] 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride (2.24 g) and 2,6-di(amino-1H-benzo[d]imidazole)pyridine (6.82 gg) and m-cresol (20 mL) were added to a 100 mL reaction bottle, nitrogen was purged for 30 min to exclude air, and then the temperature was raised to 110 ° C and stirred for 25 min to dissolve the above anhydride and diamine raw materials, followed by gradual dropwise addition of 10 mL of m-cresol solution (containing 0.2 g of isoquinoline, 20 min dropwise addition), and the temperature was raised to 140 ° C for 1 hour, and then the temperature was raised to 240 ° C for 8 hours. After the reaction was completed, the reaction solution was cooled to room temperature, and 100 mL of dimethylacetamide was added to dilute the reaction solution to reduce the viscosity of the reaction solution. Finally, the diluted reaction solution was slowly added dropwise to 2L of industrial alcohol (addition time 2h) and rapidly stirred at 1200r / min to obtain a polyimide nanofiber dispersion, which was further dialyzed three times using a 7000Da dialysis bag to remove the high boiling point solvent. Finally, the polyimide nanomaterial was freeze-dried.

Claims

1. A method for preparing a polyimide fluorescent nanomaterial, characterized in that: The specific steps include: Step 1, preparing a mixed solution using 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride, 2,6-bis(amino-1H-benzo[d]imidazole)pyridine and m-cresol; Step 2, diluting the mixed solution prepared in step 1 with dimethylacetamide; Step 3, adding industrial alcohol to the diluted solution in step 2 and stirring evenly to obtain a polyimide nanofiber dispersion; Step 4, dialyzing the polyimide nanofiber dispersion prepared in step 3, and finally freeze-drying to obtain a polyimide nanomaterial; The invention also includes an optical modification process of a polyimide nanomaterial, wherein the optical modification process of the polyimide nanomaterial is as follows: 0.5g-1g of the polyimide nanomaterial is dispersed in a mixed solution of 50 mL-100 mL of dimethylacetamide and industrial ethanol, 0.1g-0.2g of NaH is added and stirred evenly, and 0.1g-0.2g of hexafluoroacetylacetone and 0.13g-0.26g of EuCl3 are added.

2. The method for preparing the polyimide fluorescent nanomaterial according to claim 1, characterized in that: The specific process of step 1 is as follows: 2.24 g of 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride, 3.41 g-6.82 g of 2,6-bis(amino-1H-benzo[d]imidazole)pyridine and 10 mL-20 mL of m-cresol are added to a reaction bottle, and nitrogen is purged for 10 min-30 min to exclude air. Then the temperature is raised to 100°C-110°C and stirred for 10 min-25 min to dissolve all 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride and 2,6-bis(amino-1H-benzo[d]imidazole)pyridine. Subsequently, 5 mL-10 mL of m-cresol solution is added dropwise, and the temperature is raised to 120°C-140°C and maintained for 0.5 h-1 h, and then the temperature is raised to 210°C-240°C for reaction for 8 hours. After the reaction is completed, the reaction solution is lowered to room temperature to obtain the product.

3. The method for preparing the polyimide fluorescent nanomaterial according to claim 2, characterized in that: The amount of dimethylacetamide used in step 2 is 50 mL-100 mL.

4. The method for preparing the polyimide fluorescent nanomaterial according to claim 2, characterized in that: In the step 3, the amount of industrial alcohol added is 1L~2L, and the adding time is 1h~2h.

5. The method for preparing the polyimide fluorescent nanomaterial according to claim 2, characterized in that: The synthetic route of the imide nanomaterial is: 。

Citation Information

Patent Citations

  • Polyimide nano-fiber and preparation method thereof

    CN101603213A

  • In-situ preparation method for cadmium telluride / polyvinyl alcohol fluorescent fiber