Preparation method of high-strength and low-expansion polyimide flexible substrate

Through the synthesis of cellulose nanofiber modified polyimide materials, the introduction of high conjugated ring structure and cross-linking reactions has solved the shortcomings in mechanical strength and expansion properties of the polyimide substrate, and achieved high strength and low strength The expanded polyimide substrate improves the weather resistance and mechanical properties of optoelectronic devices.

CN117487213BActive Publication Date: 2024-11-22SUMII TECH (SHENZHEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311268419.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-28
Publication Date
2024-11-22
Estimated Expiration
2043-09-28

AI Technical Summary

Technical Problem

Existing polyimide substrates are difficult to meet the needs of high mechanical strength and low expansion in flexible optoelectronic devices, especially inadequate weather resistance under vacuum evaporation and physical stress.

Method used

Using cellulose nanofiber modified polyimide materials, synthesis of olefin modified cellulose nanofibers and olefin-containing end-group polyimide polymers is introduced, and highly conjugated porphyrin rings and naphthalene rings are introduced, through Hoveyda-Grubbs The catalyst is crosslinked to form a high-strength, low-expanded polyimide substrate.

Benefits of technology

The mechanical properties and thermal stability of the polyimide substrate are significantly improved, the thermal expansion coefficient is reduced, and the fracture strength and bending resistance of the film are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117487213B_ABST
    Figure CN117487213B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a high-strength, low-expansion polyimide flexible substrate, which specifically comprises the following steps: step 1, using olefin to modify cellulose nanofibers; step 2, preparing a polyimide polymer containing olefin end groups; step 3, preparing a high-strength, low-expansion polyimide substrate according to the products obtained in step 1 and step 2. The present invention uses cellulose nanofibers to modify polyimide materials, thereby obtaining a high-strength, low-expansion polyimide film material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a method for preparing a high-strength and low-expansion polyimide flexible substrate. Background Art

[0002] Polyimide is a kind of polymer material with unique structure, and its molecule has imide ring structure. Polyimide has good mechanical properties and thermal stability. With the continuous development of new polyimide polymer materials, more and more varieties are available. It is widely used in coatings, military industry, electronic appliances, and high-end optoelectronic devices.

[0003] In recent years, polyimide substrates have shown great advantages in the flexible substrates used in optoelectronic devices, meeting the high requirements of optoelectronic devices for oxygen isolation, water isolation, weather resistance, etc. On the one hand, the substrate needs to withstand high temperatures during the vacuum evaporation process of flexible optoelectronic devices; on the other hand, flexible optoelectronic devices need to withstand thousands of times of bending and folding and other physical effects during actual use, which requires the substrate to meet high mechanical strength. Therefore, how to prepare a substrate material with high strength and low expansion is an issue that the industry needs to study. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a high-strength, low-expansion polyimide flexible substrate, wherein the method adopts cellulose nanofibers to modify polyimide materials, thereby obtaining a high-strength, low-expansion polyimide film material.

[0005] The technical solution adopted by the present invention is a method for preparing a high-strength, low-expansion polyimide flexible substrate, which specifically comprises the following steps:

[0006] Step 1, using olefin to modify cellulose nanofibers;

[0007] Step 2, preparing a polyimide polymer containing olefin end groups;

[0008] Step 3, preparing a high-strength, low-expansion polyimide substrate according to the products obtained in step 1 and step 2.

[0009] The present invention is also characterized in that:

[0010] The specific process of step 1 is:

[0011] Take 0.3g-0.6g of cellulose nanocellulose, 0.5um-1um fiber length, and 20nm-40nm cellulose and ultrasonically disperse them in 10mL-20mL of dimethyl sulfoxide solution, add 1mL-2mL of NaCO3 aqueous solution, stir at room temperature for 30min, then add 0.1mL-0.2mL of allyl chloride, heat to 80℃ and continue the reaction for 12h to obtain the product.

[0012] The specific process of step 2 is:

[0013] Step 2.1, dissolve 2.68 g to 5.36 g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 3.15 g to 9.45 g of N-(4-allylphenyl)-N-(4-aminophenyl)benzene-1,4-diamine, and 0.64 g to 1.92 g of diaminotetraphenylporphyrin in 15 mL to 30 mL of m-cresol solution, and purge with nitrogen for 30 min to 60 min;

[0014] Step 2.2, add 5mL-8mL of m-cresol solution to the solution obtained in step 2.1, and heat it to 120℃-140℃ and keep it for 1h-2h, then heat it to 200℃-220℃ and react for 12h-24h, wait until the temperature drops to room temperature, add 20mL-30mL of dimethylacetamide to dilute the solution, quickly pour the diluted solution into 1L-2L of industrial alcohol to obtain a precipitate of polyimide polymer containing olefin end groups, and finally vacuum dry the product for use.

[0015] In step 2, the synthetic route of the polyimide polymer containing olefin end groups is as follows:

[0016] The specific process of step 3 is:

[0017] Step 3.1, 0.5 g to 1.5 g of polyimide polymer containing olefin end groups and 0.2 g to 0.6 g of olefin-modified cellulose nanofibers are dispersed in 20 mL to 40 mL of dimethylacetamide solution, stirred at room temperature for 30 min to 60 min, and the reaction system is purged with nitrogen for 30 min to 60 min;

[0018] Step 3.2, add 60 mg-120 mg of Hoveyda-Grubbs catalyst, react at 60°C-80°C for 24 h-30 h, dialyze with a 7000Da dialysis bag to remove the Hoveyda-Grubbs catalyst, take 50 mg of the dialyzed product and dissolve it in dimethylacetamide, stir for 12-16 hours, pour the solution into a polytetrafluoroethylene mold and vacuum dry to obtain a polyimide substrate.

[0019] The beneficial effect of the present invention is that the present invention provides a method for preparing a high-strength, low-expansion polyimide flexible substrate, which uses cellulose nanofibers to covalently modify polyimide, and at the same time introduces highly conjugated porphyrin rings and naphthalene rings into the polyimide polymer, which is beneficial to the stacking effect of the polymer chain and greatly improves the mechanical properties and thermal stability of the film. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1The stress-strain curves of the polyimide substrates prepared in Example 1 of the method for preparing a high-strength, low-expansion polyimide flexible substrate of the present invention and in Comparative Examples 1 to 3. DETAILED DESCRIPTION

[0021] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0022] The method for preparing a high-strength, low-expansion polyimide flexible substrate of the present invention specifically comprises the following steps:

[0023] 1) Olefin-modified cellulose nanofibers

[0024] Take 0.3-0.6g of cellulose nanofiber, 0.5-1um fiber length, 20-40nm cellulose, ultrasonically disperse in 10-20mL of dimethyl sulfoxide solution, add 1-2mL of NaCO3 (0.1-0.2g / mL) aqueous solution, stir at room temperature for 30min. Further add 0.1-0.2mL of allyl chloride, heat to 80℃ and continue the reaction for 12h.

[0025] 2) Preparation of polyimide polymers containing olefin end groups

[0026] Take 2.95g-5.36g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 3.15g-9.45g of N-(4-allylphenyl)-N-(4-aminophenyl)benzene-1,4-diamine, and 0.64g-1.92g of diaminotetraphenylporphyrin and dissolve them in 15mL-30mL of m-cresol solution, and purge with nitrogen for 30min-60min. Then gradually add 5-8mL of m-cresol solution (containing 0.15-0.3g of isoquinoline) dropwise, and add it over 10-15min. Then heat it to 120-140℃ and keep it for 1-2h, then heat it to 200-220℃ and react for 12-24h. When the temperature drops to room temperature, add 20-30 mL of dimethylacetamide to dilute the polymer concentration, and quickly pour the diluted solution into 1-2 L of industrial alcohol to obtain a precipitate of polyimide polymer containing olefin end groups, and finally vacuum dry the product for use.

[0027] The synthetic route of polyimide polymer containing olefin end groups is as follows:

[0028]

[0029] 3) Preparation of high-strength, low-expansion polyimide substrate

[0030] Take 0.5g-1.5g of polyimide polymer containing olefin end groups and 0.2g-0.6g of olefin-modified cellulose nanofibers and disperse them in 20-40mL of dimethylacetamide solution, stir at room temperature for 30-60min, and purge the reaction system with nitrogen for 30-60min. Add 60-120mg of Hoveyda-Grubbs catalyst (added three times, with a time interval of 8h, and each addition amount of 20-40mg), and react at 60℃~80℃ for 24~30h. After the reaction, use a 7000Da dialysis bag to dialyze to remove the Hoveyda-Grubbs catalyst. Take 50mg of the dialyzed product and dissolve it in dimethylacetamide, stir for 12~16 hours, pour the solution into a 8cmx8cm polytetrafluoroethylene mold and vacuum dry it to obtain a high-strength, low-expansion polyimide substrate.

[0031] Example 1

[0032] 1) Olefin-modified cellulose nanofibers

[0033] Take 0.3 g of cellulose nanofiber, 0.5 μm fiber length, 20 nm cellulose, ultrasonically disperse it in 10 mL of dimethyl sulfoxide solution, add 1 mL of NaCO3 (0.1 g / mL) aqueous solution, stir at room temperature for 30 min, further add 0.1 mL of allyl chloride, heat to 80 ° C and continue the reaction for 12 h.

[0034] 2) Preparation of polyimide polymers containing olefin end groups

[0035] Take 2.95g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 3.15g of N-(4-allylphenyl)-N-(4-aminophenyl)benzene-1,4-diamine, and 0.64g of diaminotetraphenylporphyrin and dissolve them in 15mL of m-cresol solution, and purge with nitrogen for 30min. Then gradually add 5mL of m-cresol solution (containing 0.15g of isoquinoline) dropwise, and add it in 10min, and heat it to 120℃ and keep it for 1h, then heat it to 200℃ and react for 12h. When the temperature drops to room temperature, add 20mL of dimethylacetamide to dilute the polymer concentration, and quickly pour the diluted solution into 1L of industrial alcohol to obtain a precipitate of polyimide polymer containing olefin end groups, and finally vacuum dry it to obtain the product for standby use. In Example 1, in the chemical structure formula of the above-mentioned synthetic route corresponding to the prepared polyimide polymer containing olefin end groups, x:y=10:1.

[0036] 3) Preparation of high-strength, low-expansion polyimide substrate

[0037] Take 0.5g of polyimide polymer containing olefin end groups and 0.2g of olefin-modified cellulose nanofibers and disperse them in 20mL of dimethylacetamide solution, stir at room temperature for 30min, and purge the reaction system with nitrogen for 30min. Add 60mg of Hoveyda-Grubbs catalyst (added three times, with a time interval of 8h, and 20mg added each time), and react at 60℃ for 24h. After the reaction, use a 7000Da dialysis bag to dialyze and remove the Hoveyda-Grubbs catalyst. Take 50mg of the dialyzed product and dissolve it in dimethylacetamide, stir for 12 hours, pour the solution into a 8cm x 8cm polytetrafluoroethylene mold and vacuum dry it to obtain a high-strength, low-expansion polyimide substrate.

[0038] Comparative Example 1 (No Cellulose Nanofibers Added to the Substrate)

[0039] Take polyimide polymer (0.5g) containing olefin end groups and disperse it in 20mL dimethylacetamide solution, stir at room temperature for 30min, and purge the reaction system with nitrogen for 30min. Add 60mg of Hoveyda-Grubbs catalyst (added three times, with a time interval of 8h, and 20mg added each time), and react at 60℃ for 24h. After the reaction, use a 7000Da dialysis bag to dialyze to remove the Hoveyda-Grubbs catalyst. Take 50mg of the dialyzed product and dissolve it in dimethylacetamide, stir for 12 hours, pour the solution into a 8cm x 8cm polytetrafluoroethylene mold and vacuum dry it to obtain a high-strength, low-expansion polyimide substrate.

[0040] Comparative Example 2 (No polymerization catalyst Hoveyda-Grubbs was added during substrate preparation, catalytic crosslinking)

[0041] Take 0.5g of polyimide polymer containing olefin end groups and 0.2 of olefin-modified cellulose nanofibers and disperse them in 20mL of dimethylacetamide solution, stir at room temperature for 30min, and purge the reaction system with nitrogen for 30min. React at 60℃ for 24h. Then dialyze with a 7000Da dialysis bag. Take 50mg of the dialyzed product and dissolve it in dimethylacetamide, stir for 12 hours, pour the solution into a 8cm x 8cm polytetrafluoroethylene mold and vacuum dry it to obtain a high-strength, low-expansion polyimide substrate.

[0042] Comparative Example 3 (No porphyrin component is added to the polyimide polymer)

[0043] Take 2.68g of 1,4,5,8-naphthalenetetracarboxylic anhydride and 3.15g of N-(4-allylphenyl)-N-(4-aminophenyl)benzene-1,4-diamine and dissolve them in 15mL of m-cresol solution, and purge with nitrogen for 30min. Then gradually add 5mL of m-cresol solution (containing 0.15g of isoquinoline) dropwise, and the addition is completed in 10min. The temperature is raised to 120℃ and maintained for 1h, and then raised to 200℃ for reaction for 12 hours. When the temperature drops to room temperature, add 20mL of dimethylacetamide to dilute the polymer concentration, and quickly pour the diluted solution into 1L of industrial alcohol to obtain a precipitate of polyimide polymer containing olefin end groups, and finally vacuum dry the product for use.

[0044] Take 0.5g of polyimide polymer containing olefin end groups and 0.2 of olefin-modified cellulose nanofibers and disperse them in 20mL of dimethylacetamide solution, stir at room temperature for 30min, and purge the reaction system with nitrogen for 30min. Add 60mg of Hoveyda-Grubbs catalyst (added three times, with a time interval of 8h, and 20mg added each time), and react at 60℃ for 24h. After the reaction, use a 7000Da dialysis bag to dialyze and remove the Hoveyda-Grubbs catalyst. Take 50mg of the dialyzed product and dissolve it in dimethylacetamide, stir for 12 hours, pour the solution into a 8cm x 8cm polytetrafluoroethylene mold and vacuum dry it to obtain a high-strength, low-expansion polyimide substrate.

[0045] Results and Discussion

[0046] Table 1 below shows the mechanical properties and thermal stability results of the polyimide substrates prepared in Example 1 and Comparative Examples 1 to 3:

[0047] Table 1

[0048]

[0049] As shown in Table 1, the thermal expansion coefficient of the polyimide substrate in Example 1 and Comparative Example 2 is relatively low (only 1.6 x 10 -6 -1.9x 10 -6 K -1 ), because cellulose nanofibers and highly conjugated naphthalene and porphyrin rings are introduced into the substrate structure, and the polyimide molecules are closely packed. The high thermal expansion coefficient in Comparative Example 1 is due to the lack of cellulose nanofibers, a component with a low thermal expansion coefficient. The thermal expansion coefficient of Comparative Example 3 is the highest, due to the lack of large conjugated porphyrin molecules, which is not conducive to the stacking of polyimide molecules.

[0050] like Figure 1As shown, Example 1 has a higher breaking strength and a lower breaking elongation, while Comparative Example 1 has a lower breaking strength and a higher breaking elongation; the main reason is that the presence of cellulose nanofibers has a mechanical strengthening effect; and the covalent bond between cellulose nanofibers and polyimide polymers plays a cross-linking role. At the same time, Comparative Example 2 is not cross-linked by Hoveyda-Grubbs catalysis, and its breaking elongation is higher.

[0051] Example 2

[0052] 1) Olefin-modified cellulose nanofibers

[0053] Take 0.5g of cellulose nanofiber, fiber length 0.8um, cellulose 30nm, ultrasonically disperse it in 15mL of dimethyl sulfoxide solution, add 1.5mL of NaCO3 (0.15g / mL) aqueous solution, stir at room temperature for 30min, further add 0.15mL of allyl chloride, heat to 80℃ and continue the reaction for 12h.

[0054] 2) Preparation of polyimide polymers containing olefin end groups

[0055] Take 4.28g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 6.84g of N-(4-allylphenyl)-N-(4-aminophenyl)benzene-1,4-diamine, and 1.48g of diaminotetraphenylporphyrin and dissolve them in 30mL of m-cresol solution, and purge with nitrogen for 50min. Then gradually add 7mL of m-cresol solution (containing 0.2g of isoquinoline) dropwise, and add it over 12min. Then heat it to 140℃ and keep it for 1.5h, and then heat it to 210℃ and react for 20h. When the temperature drops to room temperature, add 25mL of dimethylacetamide to dilute the polymer concentration, and quickly pour the diluted solution into 1.5L of industrial alcohol to obtain a precipitate of polyimide polymer containing olefin end groups, and finally vacuum dry it to obtain the product for use.

[0056] 3) Preparation of high-strength, low-expansion polyimide substrate

[0057] Take 1.2g of polyimide polymer containing olefin end groups and 0.5g of olefin-modified cellulose nanofibers and disperse them in 30mL of dimethylacetamide solution, stir at room temperature for 50min, and purge the reaction system with nitrogen for 40min. Add 90mg of Hoveyda-Grubbs catalyst (added three times, with a time interval of 8h, and 30mg added each time), and react at 70℃ for 28h. After the reaction, use a 7000Da dialysis bag to dialyze and remove the Hoveyda-Grubbs catalyst. Take 50mg of the dialyzed product and dissolve it in dimethylacetamide, stir for 14 hours, pour the solution into a 8cm x 8cm polytetrafluoroethylene mold and vacuum dry it to obtain a high-strength, low-expansion polyimide substrate.

[0058] Example 3

[0059] 1) Olefin-modified cellulose nanofibers

[0060] Take 0.6 g of cellulose nanofiber, fiber length 1.0 μm, cellulose 40 nm, ultrasonically disperse it in 20 mL of dimethyl sulfoxide solution, add 2 mL of NaCO3 (0.2 g / mL) aqueous solution, stir at room temperature for 30 min, further add 0.2 mL of allyl chloride, heat to 80 ° C and continue the reaction for 12 h.

[0061] 2) Preparation of polyimide polymers containing olefin end groups

[0062] Take 5.36g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 9.45g of N-(4-allylphenyl)-N-(4-aminophenyl)benzene-1,4-diamine, and 1.92g of diaminotetraphenylporphyrin and dissolve them in 20mL of m-cresol solution, and purge with nitrogen for 60min. Then gradually add 8mL of m-cresol solution (containing 0.3g of isoquinoline) dropwise, and add it over 15min. Then heat it to 130℃ and keep it for 2h, and then heat it to 220℃ and react for 24h. When the temperature drops to room temperature, add 30mL of dimethylacetamide to dilute the polymer concentration, and quickly pour the diluted solution into 2L of industrial alcohol to obtain a precipitate of polyimide polymer containing olefin end groups, and finally vacuum dry it to obtain the product for use.

[0063] 3) Preparation of high-strength, low-expansion polyimide substrate

[0064] Take 1.5g of polyimide polymer containing olefin end groups and 0.6g of olefin-modified cellulose nanofibers and disperse them in 40mL of dimethylacetamide solution, stir at room temperature for 60min, and purge the reaction system with nitrogen for 60min. Add 120mg of Hoveyda-Grubbs catalyst (added three times, with a time interval of 8h, and 40mg added each time), and react for 30h at 80℃. After the reaction, use a 7000Da dialysis bag to dialyze and remove the Hoveyda-Grubbs catalyst. Take 50mg of the dialyzed product and dissolve it in dimethylacetamide, stir for 16 hours, pour the solution into a 8cm x 8cm polytetrafluoroethylene mold and vacuum dry it to obtain a high-strength, low-expansion polyimide substrate.

Claims

1. A method for preparing a high-strength, low-expansion polyimide flexible substrate, characterized in that: The specific steps include: Step 1, using olefin to modify cellulose nanofibers; The specific process of step 1 is as follows: Take 0.3g-0.6g of cellulose nanofiber, 0.5um-1um fiber length, 20nm-40nm cellulose and ultrasonically disperse it in 10mL-20mL of dimethyl sulfoxide solution, add 1mL-2mL of NaCO3 aqueous solution, stir at room temperature for 30min, then add 0.1mL-0.2mL of allyl chloride and heat to 80℃. o C continued to react for 12 h to obtain; Step 2, preparing a polyimide polymer containing olefin end groups; The specific process of step 2 is as follows: Step 2.1, dissolve 2.95 g to 5.36 g of 1,4,5,8-naphthalenetetracarboxylic anhydride, 3.15 g to 9.45 g of N-(4-allylphenyl)-N-(4-aminophenyl)benzene-1,4-diamine, and 0.64 g to 1.92 g of diaminotetraphenylporphyrin in 15 mL to 30 mL of m-cresol solution, and purge with nitrogen for 30 min to 60 min; Step 2.2, add 5 mL-8 mL of m-cresol solution to the solution obtained in step 2.1, and heat to 120°C-140°C and keep for 1h-2h, then heat to 200°C-220°C and react for 12h-24h, wait until the temperature drops to room temperature, add 20 mL-30 mL of dimethylacetamide to dilute the solution, quickly pour the diluted solution into 1L-2L of industrial alcohol to obtain a precipitate of polyimide polymer containing olefin end groups, and finally vacuum dry to obtain the product for standby use; In the step 2, the synthetic route of the polyimide polymer containing olefin end groups is as follows: ; Step 3, preparing a high-strength, low-expansion polyimide substrate according to the products obtained in step 1 and step 2, the specific process of step 3 is: Step 3.1, 0.5 g to 1.5 g of polyimide polymer containing olefin end groups and 0.2 g to 0.6 g of olefin-modified cellulose nanofibers are dispersed in 20 mL to 40 mL of dimethylacetamide solution, stirred at room temperature for 30 min to 60 min, and the reaction system is purged with nitrogen for 30 min to 60 min; Step 3.2, add 60 mg-120 mg of Hoveyda-Grubbs catalyst, 60 o The reaction was carried out under C~80℃ for 24h~30h. After the reaction, the Hoveyda-Grubbs catalyst was removed by dialyzing with a 7000 Da dialysis bag. 50 mg of the dialyzed product was dissolved in dimethylacetamide and stirred for 12~16 hours. The solution was poured into a polytetrafluoroethylene mold and dried in vacuum to obtain a polyimide substrate.