Dark-colored low-roughness glazed lubricated ceramic rock slab and preparation method thereof
Through specific blank powder formula and inkjet printing technology, the problem of difficult to control the surface effect of dark-colored ceramic tiles is solved, and the preparation of low-roughness glaze lubricated ceramic rock slabs is realized, ensuring the stability of dark-colored products Production and delicate texture.
Patent Information
- Application Number
- CN202311431038.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-10-31
AI Technical Summary
The prior art is difficult to stabilize the production of dark-colored fine textured ceramic tiles, and the surface effect is difficult to control, especially the roughness Ra is difficult to be lower than 1.20μm, resulting in light-colored products on the market dominance.
Use specific blank powder formula and inkjet printing technology, including bell cover bottom glaze, bell cover top glaze, high-pressure spray permeable agent and low specific gravity spray protective glaze, combined with high-temperature firing and polishing treatment, to control surface roughness The degree is between 1.0 and 1.50 μm, and the preparation of ceramic rock slabs with dark color low-roughness glaze lubricated.
The stable production of dark-colored ceramic tiles is achieved, the surface effect is controllable, the glaze is smooth and round, and the texture is close to the fluff effect, avoiding pinholes and bubble defects and reducing production costs.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic glazed tiles, and in particular relates to a dark-colored, low-roughness glazed lubricated ceramic rock plate and a preparation method thereof. Background Art
[0002] In recent years, silk glaze, skin glaze, velvet, velvet and other ceramic tiles with delicate texture have become popular for their delicate feel, soft visual and high appearance, and are deeply loved by young consumers. Since this type of product has high requirements on the flatness of the glaze, the current main methods to solve the technical problem of uneven surface caused by spraying glaze are through pouring fine glaze and increasing the amount of flux in the glaze. However, since the current ceramic tile industry has entered the stage of "improving quality and competing for price", in order to control production costs, various types of solid waste are often mixed into the blanks. The volatilization of organic matter and impurities in these solid wastes can easily cause glaze defects, making the production process of ceramic tiles with both matte and delicate and smooth feel unstable, and the surface effect is difficult to control, especially when producing dark-colored ceramic tiles with delicate texture, defects such as pinholes and obvious orange peel on the surface are clearly displayed. Therefore, the delicate textured ceramic tiles on the market are mostly light-colored.
[0003] On the other hand, due to the extremely fierce competition in the terminal market, in order to show differentiated product characteristics, different manufacturers usually promote ceramic glazed tiles with a certain type of product with similar texture to gain market recognition. This is expressed in analogical or descriptive language. Different people have different senses and it is difficult to unify the qualitative description, which has caused chaos in the market. In the field of technology, it is also difficult to express the glaze texture in an objective way when developing glazes. The subjective expression of products brings difficulties in stable control to technology research and development and production.
[0004] Invention patent CN116023171A provides a ceramic plate with skin-friendly texture and its preparation method and application. The invention achieves a matte surface effect on the ceramic plate through the cooperation of multiple glaze layers, with a soft and comfortable visual effect, and a surface roughness of Ra = 10-15μm. The invention states that "the surface is as delicate and smooth as baby skin, and it conforms to ergonomic skin-friendly texture". In fact, when the roughness Ra = 10-15μm, the surface roughness is relatively strong, and it is more difficult to obtain the "surface as delicate and smooth as baby skin" described in the patent. After testing the surface roughness of glazes with different formulas and different textures, when Ra﹤2.0μm, the glaze texture is relatively delicate and smooth. The lower the roughness, the more delicate and smooth the surface. At present, the roughness Ra of most glazed products in the building ceramics industry is difficult to break through below 1.20μm. Summary of the invention
[0005] In view of the above-mentioned existing problems, the purpose of the present invention is to provide a method for preparing a dark-colored low-roughness glazed lubricated ceramic rock slab that can solve the problems of unstable production process of fine-textured (low surface roughness, lubricated glaze) ceramic tiles, difficult to control surface effects, and no clear indicators for glaze texture control, so as to achieve stable production process, controllable surface effects, and clear indicators for glaze texture control of dark-colored fine-textured ceramic rock slabs. Another purpose of the present invention is to provide a dark-colored low-roughness glazed lubricated ceramic rock slab that can solve the problems of rough glaze effect, rough texture, uncontrollable production stability, and difficulty in achieving large-scale production of dark-colored fine-textured ceramic inkjet products in the industry.
[0006] The technical solution of the present invention is a method for preparing the dark-colored, low-roughness, glazed and lubricated ceramic rock slab, which is special in that it comprises the following steps:
[0007] ⑴ Green body pressing: Green body powder has good fluidity, powder mass outflow time is 34-36S, repose angle is 27-30°, powder meets the requirements of the most compact powder stacking, and the stacking density is 0.95-0.98g / cm 3 , the particle size distribution is: 0.4-0.5mm particle size percentage accounts for 15-20%, 0.25-0.3mm particle size percentage accounts for 60-70%, 0.18-0.21mm particle size percentage accounts for 90-95%, and <0.17mm particle size percentage accounts for 5-10%;
[0008] (2) Drying of green body: drying temperature 160~180℃, drying time 25min;
[0009] ⑶ Base glaze: bell-shaped base glaze, glaze application amount 600g / m 2 ;
[0010] ⑷ Glaze: bell glaze, glaze amount 300g / m 2 , the glossiness of the single-sided glaze after firing is 20-25°, and the surface roughness Ra is 1.0-1.6m;
[0011] ⑸Inkjet printing: the color is dark, and the total grayscale of the ink is >200;
[0012] (6) Spray penetration enhancer: Use high pressure spray glaze to spray penetration enhancer, the spray penetration enhancer dosage is 50g / m 2 ;
[0013] ⑺ Spray protective glaze: Use high-pressure spray glaze to spray protective glaze, the specific gravity of the protective glaze is 1.20-1.32, and the glaze application amount is 200g / m 2 , use low-density spraying protective glaze to avoid excessive thickness of the glaze layer resulting in poor transparency, and ensure that the surface decoration effect of dark-colored products does not appear whitish or foggy;
[0014] ⑻ Firing: The maximum firing temperature is 1200℃, the high temperature holding time is 7-10min, the firing cycle is 70min, the glaze gloss after firing is 13-25°, the surface roughness Ra is 1.0-1.50μm, the glaze feels smooth and round, and the texture is close to the fluffy effect.
[0015] Preferably, the blank described in step (1) is polished by back-beating after pressing with a 300-mesh sponge brush. After drying, the difference in oil absorption at different positions of the blank is less than 1.5%, and the blank surface roughness is 1.7 μm < Ra < 2.8 μm.
[0016] Preferably, the chemical composition of the base glaze in step (3) consists of the following components by weight: 47.82 parts of SiO2, 17.57 parts of Al2O3, 0.21 parts of Fe2O3, 11.02 parts of CaO, 4.67 parts of MgO, 2.78 parts of K2O, 4.56 parts of Na2O, 0.07 parts of TiO2, 0.67 parts of B2O3, 3.66 parts of ZnO, and 6.97 parts of BaO.
[0017] As a preference, the glaze described in step (4) is composed of the following components by weight:
[0018] 20 parts of fluorescent screen glass slag, 10 parts of wollastonite, 5 parts of zirconium silicate, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder.
[0019] Preferably, the fluorescent screen glass slag is the recycled waste slag of fluorescent screen glass produced in the production of color television picture tubes; the molten material powder is a material obtained by mixing and calcining the raw materials of the molten material powder formula and then rolling and crushing it, and its formula is composed of the following components by weight: 5 parts of zinc oxide ore, 2 parts of barium carbonate ore, 12 parts of potassium feldspar, 36 parts of sodium feldspar, 15 parts of dolomite, 3 parts of ultrafine quartz, 11 parts of kaolin, and 10 parts of coal gangue;
[0020] The preparation method of the molten material powder comprises the following steps: weighing raw materials according to the formula of the molten material powder, mixing them evenly, calcining and melting the materials in a rotary kiln, the calcination temperature being 1200-1300° C., the calcination time being 30 min, and crushing them in a double-roll crusher after cooling to obtain the molten material powder.
[0021] Preferably, the permeation enhancer dry material in step (6) is composed of the following components by weight: 50 parts of 325 wollastonite, 30 parts of fused quartz, and 20 parts of TM frit; the preparation method of the permeation enhancer is as follows: weigh the materials according to the formula ratio of the permeation enhancer dry material, mix them evenly, pour the permeation enhancer dry material into the suspension in a ratio of permeation enhancer dry material: suspension: water = 1:1:2, and slowly stir evenly, then add water to adjust the flow rate to obtain a permeation enhancer with an Engler viscosity of 14 to 17S;
[0022] The particle size range of the TM frit is 200-300 mesh, the 325 wollastonite is wollastonite under a 325 mesh sieve, the particle size range is 325-500 mesh, and the particle size range of the fused quartz is 325-500 mesh;
[0023] The chemical composition of the TM frit is composed of the following components by weight: 55.13 parts of SiO2, 11.85 parts of Al2O3, 0.07 parts of Fe2O3, 12.17 parts of CaO, 1.79 parts of MgO, 4.04 parts of K2O, 0.51 parts of Na2O, and 14.53 parts of ZnO;
[0024] The fused quartz is amorphous (glassy) silicon dioxide formed by melting high-quality quartz raw materials (SiO2>99%) in an arc furnace or a resistance furnace, smelting at high temperature, and cooling. The melting temperature is 1695-1720°C. Compared with ordinary quartz, adding fused quartz to the glaze can reduce the melting temperature.
[0025] Preferably, the protective glaze described in step ⑺ is a glaze for obtaining a low-roughness glaze effect, and its formula consists of the following components by weight: 20 parts of fluorescent screen glass slag, 5 parts of wollastonite, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of lapis lazuli, and 46 parts of molten material powder.
[0026] Preferably, the preparation method further comprises: step (9) brush polishing: using a 400 mesh abrasive brush to brush polish the glaze surface, with a brushing pressure of 1 kg. The brushing does not change the state of the glaze surface, but removes kiln dirt or fallen dirt to further improve the surface smoothness of the glaze surface.
[0027] Another technical solution of the present invention is a dark-colored, low-roughness, glazed, lubricated ceramic rock plate prepared by the method, which is special in that it comprises the following components: a base glaze, used for pouring the base glaze in step (3); a surface glaze, used for pouring the surface glaze in step (4); a penetration enhancer, used for spraying the penetration enhancer in step (6); a protective glaze, used for spraying the protective glaze in step (7);
[0028] The chemical composition of the base glaze consists of the following components by weight: 47.82 parts of SiO2, 17.57 parts of Al2O3, 0.21 parts of Fe2O3, 11.02 parts of CaO, 4.67 parts of MgO, 2.78 parts of K2O, 4.56 parts of Na2O, 0.07 parts of TiO2, 0.67 parts of B2O3, 3.66 parts of ZnO, and 6.97 parts of BaO;
[0029] The glaze is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 10 parts of wollastonite, 5 parts of zirconium silicate, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder;
[0030] The penetration enhancer dry material is composed of the following components by weight: 50 parts of 325 wollastonite, 30 parts of fused quartz, and 20 parts of TM frit;
[0031] The protective glaze is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 5 parts of wollastonite, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder.
[0032] Preferably, the smelting material powder is composed of the following components in parts by weight: 5 parts of zinc oxide ore, 2 parts of barium carbonate, 12 parts of potassium feldspar, 36 parts of sodium feldspar, 15 parts of dolomite, 3 parts of ultrafine quartz, 11 parts of kaolin, and 10 parts of coal gangue; the chemical composition of the TM frit is composed of the following components in parts by weight: 55.13 parts of SiO2, 11.85 parts of Al2O3, 0.07 parts of Fe2O3, 12.17 parts of CaO, 1.79 parts of MgO, 4.04 parts of K2O, 0.51 parts of Na2O, and 14.53 parts of ZnO.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] ⑴ The preparation of the dark-colored, low-roughness glazed, lubricated ceramic rock slabs of the present invention adopts a glaze for obtaining a low-roughness glaze effect, the formula of which includes fluorescent screen glass slag containing a large amount of strontium silicate components, in which the carbonates and sulfates in the raw materials have been fully decomposed and the impurities are few, and a rotary kiln is used for calcination at 1200-1300°C to remove the molten material powder from the raw materials of moisture and carbon volatiles, which is beneficial to reduce the viscosity of the glaze, so that the glaze is smoother and finer after firing, and at the same time avoids the generation of defects such as bubbles and pinholes, thereby realizing the stable production of dark-colored, low-roughness glazed, lubricated ceramic rock slabs.
[0035] (2) The preparation process of the dark-colored, low-roughness, glazed and lubricated ceramic rock slab described in the present invention sprays a layer of penetration enhancer on the inkjet ink, which helps the dark ink to develop color and can reduce the amount of ink used to a certain extent. While promoting penetration and improving pattern clarity, it can also improve the problem of uneven distribution of the surface protective glaze sprayed directly on the oily ink of the decorative pattern. DETAILED DESCRIPTION
[0036] The present invention will be further described in detail below in conjunction with embodiments:
[0037] The method for preparing a dark-colored, low-roughness, glazed, lubricated ceramic rock plate comprises the following steps:
[0038] ⑴ Green body pressing: Green body powder has good fluidity, powder mass outflow time is 34-36S, repose angle is 27-30°, powder meets the requirements of the most compact powder stacking, and the stacking density is 0.95-0.98g / cm 3, the particle size distribution is: 0.4-0.5mm particle size percentage accounts for 15-20%, 0.25-0.3mm particle size percentage accounts for 60-70%, 0.18-0.21mm particle size percentage accounts for 90-95%, and <0.17mm particle size percentage accounts for 5-10%;
[0039] The blank described in step (1) is polished by back-beating after pressing with a 300-mesh sponge brush. After drying, the difference in oil absorption rate at different positions of the blank is less than 1.5%, and the blank surface roughness is 1.7 μm < Ra < 2.8 μm.
[0040] (2) Drying of green body: drying temperature 160~180℃, drying time 25min;
[0041] ⑶ Base glaze: bell-shaped base glaze, glaze application amount 600g / m 2 ;
[0042] Step (3) The chemical composition of the base glaze consists of the following components by weight: 47.82 parts of SiO2, 17.57 parts of Al2O3, 0.21 parts of Fe2O3, 11.02 parts of CaO, 4.67 parts of MgO, 2.78 parts of K2O, 4.56 parts of Na2O, 0.07 parts of TiO2, 0.67 parts of B2O3, 3.66 parts of ZnO, and 6.97 parts of BaO;
[0043] ⑷ Glaze: bell glaze, glaze amount 300g / m 2 , the glossiness of the single-sided glaze after firing is 20-25°, and the surface roughness Ra is 1.0-1.6m;
[0044] The glaze described in step (4) is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 10 parts of wollastonite, 5 parts of zirconium silicate, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder;
[0045] The fluorescent screen glass slag is the recycled waste slag of fluorescent screen glass produced in the production of color television picture tubes; the molten material powder is a material obtained by mixing and calcining the raw materials of the molten material powder formula and then rolling and crushing it, and the formula is composed of the following components by weight: 5 parts of zinc oxide ore, 2 parts of barium carbonate ore, 12 parts of potassium feldspar, 36 parts of sodium feldspar, 15 parts of dolomite, 3 parts of ultrafine quartz, 11 parts of kaolin, and 10 parts of coal gangue;
[0046] The preparation method of the molten material powder comprises: weighing the raw materials according to the formula of the molten material powder, mixing them evenly, calcining and melting the materials in a rotary kiln, the calcination temperature is 1200-1300° C., the calcination time is 30 minutes, and after cooling, crushing them in a double-roll crusher to obtain the molten material powder;
[0047] ⑸Inkjet printing: the color is dark, and the total grayscale of the ink is >200;
[0048] (6) Spray penetration enhancer: Use high pressure spray glaze to spray penetration enhancer, the spray penetration enhancer dosage is 50g / m 2 ;
[0049] Step (6) The penetration enhancer dry material is composed of the following components by weight: 50 parts of 325 wollastonite, 30 parts of fused quartz, and 20 parts of TM frit; the preparation method of the penetration enhancer is as follows: weigh the materials according to the formula ratio of the penetration enhancer dry material, mix them evenly, pour the penetration enhancer dry material into the suspension in a ratio of penetration enhancer dry material: suspension: water = 1:1:2, and slowly stir evenly, then add water to adjust the flow rate to obtain a penetration enhancer with an Engler viscosity of 14 to 17S;
[0050] The particle size range of the TM frit is 200-300 mesh, the 325 wollastonite is wollastonite under a 325 mesh sieve, the particle size range is 325-500 mesh, and the particle size range of the fused quartz is 325-500 mesh;
[0051] The chemical composition of the TM frit is composed of the following components by weight: 55.13 parts of SiO2, 11.85 parts of Al2O3, 0.07 parts of Fe2O3, 12.17 parts of CaO, 1.79 parts of MgO, 4.04 parts of K2O, 0.51 parts of Na2O, and 14.53 parts of ZnO;
[0052] The fused quartz is amorphous (glassy) silicon dioxide formed by melting high-quality quartz raw materials (SiO2>99%) in an arc furnace or a resistance furnace, smelting at high temperature, and cooling. The melting temperature is 1695-1720°C. Adding fused quartz to the glaze can reduce the melting temperature.
[0053] ⑺ Spray protective glaze: Use high-pressure spray glaze to spray protective glaze, the specific gravity of the protective glaze is 1.20-1.32, and the glaze application amount is 200g / m 2 , use low-density spraying protective glaze to avoid excessive thickness of the glaze layer resulting in poor transparency, and ensure that the surface decoration effect of dark-colored products does not appear whitish or foggy;
[0054] The protective glaze described in step (7) is a glaze for obtaining a low-roughness glaze effect, and its formula is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 5 parts of wollastonite, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder;
[0055] ⑻ Firing: The maximum firing temperature is 1200℃, the high temperature holding time is 7-10min, the firing cycle is 70min, the glaze gloss after firing is 13-25°, the surface roughness Ra is 1.0-1.50μm, the glaze feels smooth and round, and the texture is close to the fluff effect;
[0056] ⑼ Brush polishing: Use a 400-mesh abrasive brush to brush the glaze surface. The brushing pressure is 1kg. Brushing does not change the state of the glaze surface. It removes kiln dirt or fallen dirt to further improve the surface smoothness of the glaze.
[0057] A dark-colored, low-roughness, glazed, lubricated ceramic rock plate prepared according to the method comprises the following components: a base glaze, used for pouring the base glaze in step (3); a surface glaze, used for pouring the surface glaze in step (4); a penetration enhancer, used for spraying the penetration enhancer in step (6); and a protective glaze, used for spraying the protective glaze in step (7);
[0058] The chemical composition of the base glaze consists of the following components by weight: 47.82 parts of SiO2, 17.57 parts of Al2O3, 0.21 parts of Fe2O3, 11.02 parts of CaO, 4.67 parts of MgO, 2.78 parts of K2O, 4.56 parts of Na2O, 0.07 parts of TiO2, 0.67 parts of B2O3, 3.66 parts of ZnO, and 6.97 parts of BaO;
[0059] The glaze is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 10 parts of wollastonite, 5 parts of zirconium silicate, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder; the molten material powder is composed of the following components by weight: 5 parts of zinc oxide ore, 2 parts of barium carbonate ore, 12 parts of potassium feldspar, 36 parts of sodium feldspar, 15 parts of dolomite, 3 parts of ultrafine quartz, 11 parts of kaolin, and 10 parts of coal gangue; the chemical composition of the TM frit is composed of the following components by weight: 55.13 parts of SiO2, 11.85 parts of Al2O3, 0.07 parts of Fe2O3, 12.17 parts of CaO, 1.79 parts of MgO, 4.04 parts of K2O, 0.51 parts of Na2O, and 14.53 parts of ZnO;
[0060] The penetration enhancer dry material is composed of the following components by weight: 50 parts of 325 wollastonite, 30 parts of fused quartz, and 20 parts of TM frit;
[0061] The protective glaze is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 5 parts of wollastonite, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder.
[0062] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should fall within the scope of the claims of the present invention.
Claims
1. A method for preparing a dark-colored, low-roughness, glazed, lubricated ceramic rock slab, characterized in that: The following steps are involved: ⑴ Green body pressing: Green body powder has good fluidity, powder mass outflow time is 34-36S, repose angle is 27-30°, powder meets the requirements of the most compact powder stacking, and the stacking density is 0.95-0.98g / cm 3 , the particle size distribution is: 0.4-0.5mm particle size percentage accounts for 15-20%, 0.25-0.3mm particle size percentage accounts for 60-70%, 0.18-0.21mm particle size percentage accounts for 90-95%, and <0.17mm particle size percentage accounts for 5-10%; (2) Drying of green body: drying temperature 160~180℃, drying time 25min; ⑶ Base glaze: bell-shaped base glaze, glaze application amount 600g / m 2 ; ⑷ Glaze: bell glaze, glaze amount 300g / m 2 , the glossiness of the single-sided glaze after firing is 20-25°, and the surface roughness Ra: 1.0-1.6 microns; ⑸Inkjet printing: the color is dark, and the total grayscale of the ink is >200; (6) Spray penetration enhancer: Use high pressure spray glaze to spray penetration enhancer, the spray penetration enhancer dosage is 50g / m 2 ; ⑺ Spray protective glaze: Use high-pressure spray glaze to spray protective glaze, the specific gravity of the protective glaze is 1.20-1.32, and the glaze application amount is 200g / m 2 , use low specific gravity to spray protective glaze to avoid poor transparency caused by too thick glaze layer, and ensure that the surface decoration effect of dark-colored products is not whitish and hazy; the protective glaze described in step ⑺ is a glaze for obtaining a low-roughness glaze effect, and its formula is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 5 parts of wollastonite, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder; ⑻ Firing: The maximum firing temperature is 1200℃, the high temperature holding time is 7-10min, the firing cycle is 70min, the glaze gloss after firing is 13-25°, the surface roughness Ra is 1.0-1.50μm, the glaze feels smooth and round, and the texture is close to the fluffy effect.
2. The method for preparing a dark-colored, low-roughness, glazed, lubricated ceramic rock slab according to claim 1, characterized in that: The blank described in step (1) is polished by back-beating after pressing with a 300-mesh sponge brush grinding block. After drying, the difference in oil absorption rate at different positions of the blank is less than 1.5%, and the blank surface roughness is 1.7 μm < Ra < 2.8 μm.
3. The method for preparing a dark-colored, low-roughness, glazed, lubricated ceramic rock slab according to claim 1, characterized in that: Step (3) The chemical composition of the base glaze consists of the following components by weight: 47.82 parts of SiO2, 17.57 parts of Al2O3, 0.21 parts of Fe2O3, 11.02 parts of CaO, 4.67 parts of MgO, 2.78 parts of K2O, 4.56 parts of Na2O, 0.07 parts of TiO2, 0.67 parts of B2O3, 3.66 parts of ZnO, and 6.97 parts of BaO.
4. The method for preparing a dark-colored, low-roughness, glazed, lubricated ceramic rock slab according to claim 1, characterized in that: The glaze described in step (4) is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 10 parts of wollastonite, 5 parts of zirconium silicate, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder.
5. The method for preparing a dark-colored, low-roughness, glazed, lubricated ceramic rock slab according to claim 4, characterized in that: The fluorescent screen glass slag is the recycled waste slag of fluorescent screen glass produced in the production of color television picture tubes; the molten material powder is a material obtained by mixing and calcining the raw materials of the molten material powder formula and then rolling and crushing it, and the formula is composed of the following components by weight: 5 parts of zinc oxide ore, 2 parts of barium carbonate ore, 12 parts of potassium feldspar, 36 parts of sodium feldspar, 15 parts of dolomite, 3 parts of ultrafine quartz, 11 parts of kaolin, and 10 parts of coal gangue; The preparation method of the molten material powder comprises the following steps: weighing raw materials according to the formula of the molten material powder, mixing them evenly, calcining and melting the materials in a rotary kiln, the calcination temperature being 1200-1300° C., the calcination time being 30 min, and crushing them in a double-roll crusher after cooling to obtain the molten material powder.
6. The method for preparing a dark-colored, low-roughness, glazed, lubricated ceramic rock slab according to claim 1, characterized in that: Step (6) The penetration enhancer dry material is composed of the following components by weight: 50 parts of 325 wollastonite, 30 parts of fused quartz, and 20 parts of TM frit; the preparation method of the penetration enhancer is as follows: weigh the materials according to the formula ratio of the penetration enhancer dry material, mix them evenly, pour the penetration enhancer dry material into the suspension in a ratio of penetration enhancer dry material: suspension: water = 1:1:2, and slowly stir evenly, then add water to adjust the flow rate to obtain a penetration enhancer with an Engler viscosity of 14 to 17S; The particle size range of the TM frit is 200-300 mesh, the 325 wollastonite is wollastonite under a 325 mesh sieve, the particle size range is 325-500 mesh, and the particle size range of the fused quartz is 325-500 mesh; The chemical composition of the TM frit is composed of the following components by weight: 55.13 parts of SiO2, 11.85 parts of Al2O3, 0.07 parts of Fe2O3, 12.17 parts of CaO, 1.79 parts of MgO, 4.04 parts of K2O, 0.51 parts of Na2O, and 14.53 parts of ZnO; The fused quartz is a non-crystalline glassy silicon dioxide formed by melting high-quality quartz raw material SiO2>99% in an arc furnace or a resistance furnace, smelting at high temperature, and cooling, and the melting temperature is 1695-1720°C; compared with ordinary quartz, adding fused quartz to the glaze can reduce the melting temperature.
7. The method for preparing a dark-colored, low-roughness, glazed, lubricated ceramic rock slab according to claim 1, characterized in that: The preparation method also includes: step (9) brush polishing: using a 400-mesh grinding brush to brush polish the glaze surface, the brushing pressure is 1kg, the brushing does not change the glaze state, the kiln dirt or fallen dirt is removed, and the surface flatness of the glaze is further improved.
8. A dark-colored, low-roughness, glazed, lubricated ceramic rock plate prepared according to the method of claim 1, characterized in that: The method comprises the following components: a base glaze, which is used for pouring the base glaze in step (3); and a top glaze, which is used for pouring the top glaze in step (4); A penetration enhancer, used for printing the penetration enhancer in step (6); Protective glaze, used for spraying protective glaze in step ⑺; The chemical composition of the base glaze consists of the following components by weight: 47.82 parts of SiO2, 17.57 parts of Al2O3, 0.21 parts of Fe2O3, 11.02 parts of CaO, 4.67 parts of MgO, 2.78 parts of K2O, 4.56 parts of Na2O, 0.07 parts of TiO2, 0.67 parts of B2O3, 3.66 parts of ZnO, and 6.97 parts of BaO; The glaze is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 10 parts of wollastonite, 5 parts of zirconium silicate, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder; The penetration enhancer dry material is composed of the following components by weight: 50 parts of 325 wollastonite, 30 parts of fused quartz, and 20 parts of TM frit; the chemical composition of the TM frit is composed of the following components by weight: 55.13 parts of SiO2, 11.85 parts of Al2O3, 0.07 parts of Fe2O3, 12.17 parts of CaO, 1.79 parts of MgO, 4.04 parts of K2O, 0.51 parts of Na2O, and 14.53 parts of ZnO; The 325 wollastonite is wollastonite under a 325 mesh sieve, and the particle size range is 325 mesh to 500 mesh; the particle size range of the TM frit is 200 mesh to 300 mesh, and the particle size range of the fused quartz is 325 mesh to 500 mesh; The protective glaze is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 5 parts of wollastonite, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder.
9. The dark-colored, low-roughness, glazed, lubricated ceramic rock plate prepared by the method according to claim 8, characterized in that: The smelting material powder consists of the following components by weight: 5 parts of zinc oxide ore, 2 parts of barium carbonate, 12 parts of potassium feldspar, 36 parts of sodium feldspar, 15 parts of dolomite, 3 parts of ultrafine quartz, 11 parts of kaolin and 10 parts of coal gangue.