A method for preparing bio-based amine compounds by converting marine biomass

Through the two-step or one-step method of marine biomass combined with the acidic cocatalysis of precious metal catalysts, the problem of high energy consumption of chitin in industrial ammonia synthesis is solved, and high-efficiency preparation of bio-based amine compounds is achieved, which improves chitin The conversion rate and selective production of amines promote high-value utilization of seafood waste and nitrogen circulation.

CN117551056BActive Publication Date: 2024-11-08GUANGDONG UNIV OF TECH +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311525872.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-15
Publication Date
2024-11-08
Estimated Expiration
2043-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently use chitin to prepare high-yield nitrogen-containing chemicals, especially amine compounds, and it is often dependent on the high-energy-consuming ammonia synthesis process in the industry.

Method used

Using the two-step or one-step method of marine biomass, the mixture of nitric acid aqueous solution, activated carbon, melamine and noble metal catalysts, acid cocatalysis and hydroxide treatment are performed to selectively remove the oxygen-containing groups of chitin and convert them into Highly efficient bio-based amine compounds.

Benefits of technology

It realizes the direct acquisition of high-efficiency bio-based amine compounds from chitin, avoids the high-energy ammonia synthesis process, improves the conversion rate of chitin and selective production of amines, and promotes the high waste of crustacean seafood. Value utilization and nitrogen circulation are opened up.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117551056B_ABST
    Figure CN117551056B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing bio-based amine compounds by converting marine biomass; the method removes oxygen elements from chitin through a loaded ruthenium catalyst and a phosphoric acid co-catalyst, while retaining the amino groups in chitin, and converts chitin into biogenic amines; by optimizing the catalyst, the amino groups are retained through the co-catalyst, thereby improving the conversion rate of chitin and achieving selective production of amines. The method can achieve high-value utilization of crustacean seafood waste and reduce the use of high-energy-consuming synthetic ammonia.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical engineering technology, relates to a catalytic conversion technology of biomass, and particularly relates to a method for preparing bio-based amine compounds by catalytic conversion of marine biomass chitin. Background Art

[0002] Chitin is a raw material for "nitrogen-rich chemicals for pharmaceuticals, cosmetics, textiles, water treatment, household cleaners, soaps and CO2 sequestration". The main difference of chitin compared to cellulose is that it has biologically fixed nitrogen on its side chains. Therefore, N-containing chemicals can be directly obtained from chitin, which are usually produced industrially starting from the energy-intensive ammonia synthesis.

[0003] Chitin is a suitable raw material for the preparation of nitrogen-containing chemicals. Although the use of chitin as a raw material for renewable organic nitrogen-containing compounds has been proposed since 2015, high-yield amine compounds have not yet been achieved. The key challenge is that the amide group is easily detached from the main chain. However, the selective deoxygenation of chitin or its monomer NAG is of interest for the synthesis of commodity chemicals such as amines. To the best of our knowledge, there are very limited studies on the selective deoxygenation of chitin or NAG to amines. For example, NAG is partially deoxygenated by pyrolysis to produce chemicals such as 3-acetamidofuran, 3-acetamido-5-acetylfuran (3A5AF), acetamidoacetaldehyde, pyrazines, pyridines, etc., but the yield is relatively low (J. Anal. Appl. Pyrolysis 1984, 7, 91–100; J. Agric. Food Chem. 1998, 46, 3207–3209). On the other hand, gold nanoparticles dispersed on alkaline supports can partially oxidize NAG in water to produce N-acetylglucosamine with a yield of up to 95% (ChemSusChem 2013, 6, 2259–2262). In recent years, the pharmaceutical industry has developed new processes for converting NAG into platform chemical building blocks, such as 3-acetamido-5-acetylfuran (3A5AF) for the synthesis of the anticancer drug alkaloid Proximicin A (ChemSusChem 2018, 11, 532–535; ChemSusChem 2012, 5, 1767–1772). Under microwave conditions (220°C, 15min), using dimethylacetamide as solvent, the yield of 3A5AF increased from 2% (J. Anal. Appl. Pyrolysis 1984, 7, 91–100) to 58% (ChemSusChem 2012, 5, 1767–1772). If the reaction takes place in an imidazolium ionic liquid, the yield of 3A5AF can reach 60% (RSCAdv. 2012, 2, 4642–4644). However, the market for specialty chemicals like 3A5AF is small and can only consume very limited chitin raw materials.

[0004] In recent years, low-yield pyrroles were found in the process of converting chitin to acetic acid, with a yield of only 12 mol% (ACS Sustain. Chem. Eng. 2016, 4, 3912–3920). The amide / amino-substituted sugar alcohols, C2-C4 polyols, and N-acetyl monoethanolamine (NMEA) produced by the hydrogenation reaction of NAG on precious metal catalysts have poor selectivity due to the lack of protection of the amino group of NAG (Green Chem. 2015, 17, 1024–1031). As a result, the deamination reaction dominates, leading to the production of polyols. Therefore, in the process of converting chitin to amines on precious metal catalysts, an effective catalytic strategy to protect the amino group must be adopted. Summary of the invention

[0005] The present invention provides a method for directly obtaining nitrogen-containing chemicals from chitin, because chitin side chains contain biologically fixed nitrogen and nitrogen-containing chemicals are usually produced industrially starting from high-energy-consuming ammonia synthesis.

[0006] The present invention provides a new method for directly obtaining nitrogen-containing chemicals from chitin, aiming at the fact that the side chain of chitin contains biologically fixed nitrogen, thereby avoiding the problem of using high-energy-consuming ammonia synthesis to produce nitrogen-containing chemicals in industry, while retaining the hydrocarbon components of the chitin skeleton.

[0007] To achieve the above purpose, the present invention adopts the following two technical solutions:

[0008] 1. A method for preparing bio-based amine compounds by two-step conversion of marine biomass, comprising the following steps:

[0009] 1) Mix 5% to 68% nitric acid aqueous solution with activated carbon (Ac) equivalent to 0.05 to 0.5 times the mass of the nitric acid aqueous solution, and stir at 10 to 1000 pm for 0.5 to 48 hours at 20 to 100 ° C to obtain Ac-HNO3; grind Ac-HNO3 and melamine (melamine) in a mass ratio of 1:10 to 10:1, place them in a tube furnace, and use a nitrogen flow rate of 0.1 to 200 mL / min. Then, heat the temperature from 30 ° C to 600 ° C, maintain it for 120 to 480 minutes, and then cool it down to obtain the catalyst carrier Ac-HNO3-melamine; grind Ac and melamine (melamine) in a mass ratio of 10:1 to 1:10, place them in a tube furnace, and use a nitrogen flow rate of 0.1 to 200 mL / min. The temperature is raised from 30°C to 400-800°C, maintained for 120-480 minutes, and then cooled to obtain the catalyst carrier Ac-melamine; RuCl3 is dissolved in acetone and mixed with the catalyst carrier Ac, Ac-HNO3, Ac-melamine, and Ac-HNO3-melamine respectively, stirred until the liquid is dry, and dried to obtain RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, and RuCl3 / Ac-HNO3-melamine respectively; RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, and RuCl3 / Ac-HNO3-melamine are hydrolyzed with sodium hydroxide to obtain RuO x / Ac、RuO x / Ac-HNO3、RuO x / Ac-melamine、RuO x / Ac-HNO3-melamine, or by reducing RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, RuCl3 / Ac-HNO3-melamine with sodium borohydride equivalent to 1 to 10 times the mass of Ru to obtain Ru / Ac, Ru / Ac-HNO3, Ru / Ac-melamine, Ru / Ac-HNO3-melamine respectively;

[0010] 2) placing 45-95% water, 1-60% phosphoric acid (H3PO4), and 0.5-30% chitin in a reaction kettle, and reacting for 1-12 hours at 80-150°C and 0.1-10 MPa nitrogen;

[0011] 3) After the reaction liquid is cooled, 0.1-30% of one or more of the above catalysts is added, and the mixture is put into the reaction kettle again, and reacted for 1-12 hours at 200-250° C. and 1.0-3.0 MPa of hydrogen to obtain a phosphorylated organic amine, and the yield of the organic amine is 1-99%.

[0012] 2. A method for preparing bio-based amine compounds by one-step conversion of marine biomass, comprising the following steps:

[0013] 1) Mix 5% to 68% nitric acid aqueous solution with activated carbon (Ac) equivalent to 0.05 to 0.5 times the mass of the nitric acid aqueous solution, and stir at 10 to 1000 pm for 0.5 to 48 hours at 20 to 100°C to obtain Ac-HNO3; grind Ac-HNO3 and melamine in a mass ratio of 1:10 to 10:1, place them in a tube furnace, and use a nitrogen flow rate of 0.1 to 200 mL / min. Then, raise the temperature from 25°C to 600°C, maintain for 120 to 480 minutes, and cool down to obtain the catalyst carrier Ac-HNO3-melamine; grind Ac and melamine in a mass ratio of 10:1 to 1:10, place them in a tube furnace, and use a nitrogen flow rate of 0.1 to 200 mL / min. Then, raise the temperature from 25°C to 600°C, maintain for 120 to 480 minutes, and cool down to obtain the catalyst carrier Ac-HNO3-melamine. The catalyst carrier Ac-melamine is obtained by heating from 25°C to 400-800°C and maintaining for 120-480 minutes, and then cooling down; RuCl3 is dissolved in acetone and mixed with the catalyst carrier Ac, Ac-HNO3, Ac-melamine, and Ac-HNO3-melamine respectively, and stirred until the liquid is dry, and then dried to obtain RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, and RuCl3 / Ac-HNO3-melamine respectively; RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, and RuCl3 / Ac-HNO3-melamine are hydrolyzed with sodium hydroxide to obtain RuO x / Ac、RuO x / Ac-HNO3、RuO x / Ac-melamine、RuO x / Ac-HNO3-melamine, or by reducing RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, RuCl3 / Ac-HNO3-melamine with sodium borohydride equivalent to 1 to 10 times the mass of Ru to obtain Ru / Ac, Ru / Ac-HNO3, Ru / Ac-melamine, Ru / Ac-HNO3-melamine respectively;

[0014] 2) 45-95% water, 1-60% phosphoric acid (H3PO4), 0.5-30% chitin, and 0.1-30% of one or more of the above catalysts are placed in a reaction kettle, and reacted at 200-250° C. and 1.0-3.0 MPa hydrogen for 1-12 hours to obtain a phosphorylated organic amine, and the yield of the organic amine is 1-99%.

[0015] Preferably, the mass fraction of chitin in the reaction system is 1.5% to 20%, the mass fraction of phosphoric acid is 1 to 20%, and the mass fraction of the catalyst is 0.1 to 5%.

[0016] The catalyst may be RuO x / Ac、RuO x / Ac-HNO3、RuO x / Ac-melamine、RuO x / Ac-HNO3-melamine, Ru / Ac, Ru / Ac-HNO3, Ru / Ac-melamine, and one or more of Ru / Ac-HNO3-melamine.

[0017] The catalyst can be reused after filtering, and the organic amine can be neutralized by a common base to become a free state, and a mixture of organic amines can be obtained by simple distillation.

[0018] The present invention adopts the above technical solution, which has the following advantages:

[0019] (1) In order to solve the problem of high energy consumption in the industrial synthesis of organic amines from ammonia, we proposed to use the nitrogen fixed by chitin in the ocean to achieve green production of organic amines. We developed a new catalytic method to hydrolyze chitin into monomer NAG by acidic co-catalyst, and selectively remove the oxygen-containing groups of NAG on the supported precious metal catalyst while retaining the amino groups in NAG, thus converting NAG into biogenic amines.

[0020] (2) By optimizing the catalytic reaction system, the amino group is retained by the co-catalyst, thereby improving the conversion rate of chitin and achieving the selective production of amines. By developing multiple reaction pathways for chitin to generate different amines, the high-value utilization of chitin can be achieved. These discoveries can achieve high-value utilization of crustacean seafood waste and open up the nitrogen cycle on Earth. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 : Amine yields of chitin catalyzed by eight different catalysts (two-step process).

[0022] Figure 2 : Amine yields of chitin catalyzed by eight different catalysts (one-step process). DETAILED DESCRIPTION

[0023] The present invention is described in detail below by way of examples.

[0024] Example 1

[0025] Preparation of 2.5wt%RuO x / Ac catalyst requires three steps:

[0026] The first step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0027] In the second step, 0.78 g of catalyst carrier Ac is mixed with ruthenium trichloride (RuCl3) acetone solution, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac.

[0028] In the third step, 2.5 wt% RuCl3 / Ac was hydrolyzed by sodium hydroxide (NaOH) to obtain 2.5 wt% RuO x / Ac. First, take 0.325g of 2.5wt% RuCl3 / Ac and add it to 40mL of water and stir. Then take 0.014g of NaOH and mix it with 20mL of water. Then slowly add the sodium hydroxide aqueous solution to the 2.5wt% RuCl3 / Ac suspension within 10min. Filter the obtained liquid and dry the obtained solid to obtain 2.5wt% RuO x / Ac catalyst.

[0029] We use a two-step reaction method:

[0030] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), and 0.3047 g of chitin was added, and the mixture was placed in a reactor and reacted at 100°C and 0.5 MPa of nitrogen for 2 hours.

[0031] After cooling, add 0.1 g 2.5 wt% RuO x / Ac catalyst, put it into the reactor again, and react at 250°C and 3.0MPa hydrogen for 2 hours to obtain organic amine.

[0032] Example 2

[0033] There are four steps to prepare 2.5wt% RuOx / Ac-HNO3 catalyst:

[0034] The first step is to make Ac-HNO3. First, mix 33.38mL of concentrated nitric acid with 66mL of water to obtain 8mol / L nitric acid solution. Then take 100mL of 8mol / L nitric acid solution and mix it with 10g of 400-mesh activated carbon after screening, and stir it at 80℃ and 300rpm for 8h. After stirring, filter the liquid and dry it to obtain Ac-HNO3.

[0035] The second step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0036] In the third step, 0.78 g of the catalyst carrier Ac-HNO3 is mixed with the ruthenium trichloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-HNO3.

[0037] The fourth step is to hydrolyze 2.5 wt% RuCl3 / Ac-HNO3 with sodium hydroxide (NaOH) to obtain 2.5 wt% RuO x / Ac-HNO3. First, take 0.325g of 2.5wt% RuCl3 / Ac-HNO3 and add it to 40mL of water and stir. Then take 0.014g of NaOH and mix it with 20mL of water. Then slowly add the sodium hydroxide aqueous solution to the 2.5wt% RuCl3 / Ac-HNO3-melamine suspension within 10min. Filter the obtained liquid, and then dry the obtained solid to obtain 2.5wt% RuO x / Ac-HNO3 catalyst.

[0038] We use a two-step reaction method:

[0039] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), and 0.3047 g of chitin was added, and the mixture was placed in a reactor and reacted at 100°C and 0.5 MPa of nitrogen for 2 hours.

[0040] After cooling, add 0.1 g 2.5 wt% RuO x / Ac-HNO3-melamine catalyst is put into the reactor again and reacted at 250°C and 3.0MPa hydrogen for 2 hours to obtain organic amine.

[0041] Example 3

[0042] Preparation of 2.5wt%RuO x / Ac-melamine catalyst requires four steps:

[0043] In the first step, 1.5 g of Ac and 1.5 g of melamine are mixed and ground and then put into a porcelain boat, and the porcelain boat containing the mixture is placed in a tube furnace, and nitrogen is passed through for 10 minutes, and then the temperature is raised from 25°C to 600°C over 190 minutes, and then maintained at 600°C for 120 minutes. After cooling, the catalyst carrier Ac-melamine can be obtained.

[0044] The second step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0045] In the third step, 0.78 g of the catalyst carrier Ac-melamine is mixed with the ruthenium chloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-melamine.

[0046] The fourth step is to hydrolyze 2.5 wt% RuCl3 / Ac-melamine with sodium hydroxide (NaOH) to obtain 2.5 wt% RuO x / Ac-melamine. First, take 0.325g of 2.5wt% RuCl3 / Ac-melamine and add it to 40mL of water and stir. Then take 0.014g of NaOH and mix it with 20mL of water. Then slowly add the sodium hydroxide aqueous solution to the 2.5wt% RuCl3 / Ac-melamine suspension within 10min. Filter the obtained liquid, and then dry the obtained solid to obtain 2.5wt% RuO x / Ac-melamine catalyst.

[0047] We use a two-step reaction method:

[0048] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), and 0.3047 g of chitin was added, and the mixture was placed in a reactor and reacted at 100°C and 0.5 MPa of nitrogen for 2 hours.

[0049] After cooling, add 0.1 g 2.5 wt% RuO x / Ac-melamine catalyst is put into the reactor again and reacted at 250°C and 3.0MPa hydrogen for 2 hours to obtain organic amine.

[0050] Example 4

[0051] Preparation of 2.5wt%RuO x / Ac-HNO3-melamine catalyst requires five steps:

[0052] The first step is to make Ac-HNO3. First, mix 33.38mL of concentrated nitric acid with 66mL of water to obtain 8mol / L nitric acid solution. Then take 100mL of 8mol / L nitric acid solution and mix it with 10g of 400-mesh activated carbon after screening, and stir it at 80℃ and 300rpm for 8h. After stirring, filter the liquid and dry it to obtain Ac-HNO3.

[0053] In the second step, 1.5 g of Ac-HNO3 and 1.5 g of melamine were mixed and ground and then put into a porcelain boat, and the porcelain boat containing the mixture was placed in a tube furnace, and nitrogen was first passed for 10 minutes, and then the temperature was raised from 25°C to 600°C over 190 minutes, and then maintained at 600°C for 120 minutes. After cooling, the catalyst carrier Ac-HNO3-melamine was obtained.

[0054] The third step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0055] In the fourth step, 0.78 g of the catalyst carrier Ac-HNO3-melamine is mixed with the ruthenium trichloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is dried, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-HNO3-melamine.

[0056] The fifth step is to hydrolyze 2.5wt%RuCl3 / Ac-HNO3-melamine with sodium hydroxide (NaOH) to obtain 2.5wt%RuO x / Ac-HNO3-melamine. First, take 0.325g of 2.5wt% RuCl3 / Ac-HNO3-melamine and add it to 40mL of water and stir. Then take 0.014g of NaOH and mix it with 20mL of water. Then slowly add the sodium hydroxide aqueous solution to the 2.5wt% RuCl3 / Ac-HNO3-melamine suspension within 10min. Filter the obtained liquid, and then dry the obtained solid to obtain 2.5wt% RuO x / Ac-HNO3-melamine catalyst.

[0057] We use a two-step reaction method:

[0058] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), and 0.3047 g of chitin was added, and the mixture was placed in a reactor and reacted at 100°C and 0.5 MPa of nitrogen for 2 hours.

[0059] After cooling, add 0.1 g 2.5 wt% RuO x / Ac-HNO3-melamine catalyst is put into the reactor again and reacted at 250°C and 3.0MPa hydrogen for 2 hours to obtain organic amine.

[0060] Example 5

[0061] There are three steps to prepare 2.5wt%Ru / Ac catalyst:

[0062] The first step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0063] In the second step, 0.78 g of catalyst carrier Ac is mixed with ruthenium trichloride (RuCl3) acetone solution, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac.

[0064] The third step is to reduce 2.5wt% RuCl3 / Ac with sodium borohydride to obtain 2.5wt% Ru / Ac. First, 0.325g of 2.5wt% RuCl3 / Ac is added to 40mL of water and stirred. Then 0.014g of sodium borohydride is mixed with 20mL of water. Then, the sodium borohydride aqueous solution is slowly added dropwise to the 2.5wt% RuCl3 / Ac suspension within 10 minutes. The obtained liquid is filtered, and the obtained solid is dried to obtain a 2.5wt% Ru / Ac catalyst.

[0065] We use a two-step reaction method:

[0066] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), and 0.3047 g of chitin was added, and the mixture was placed in a reactor and reacted at 100°C and 0.5 MPa of nitrogen for 2 hours.

[0067] After cooling, 0.1 g of 2.5 wt% Ru / Ac catalyst was added, and the mixture was put into the reactor again. The mixture was reacted at 250° C. and 3.0 MPa of hydrogen for 2 hours to obtain an organic amine.

[0068] Example 6

[0069] There are four steps to prepare 2.5wt%Ru / Ac-HNO3 catalyst:

[0070] The first step is to make Ac-HNO3. First, mix 33.38mL of concentrated nitric acid with 66mL of water to obtain 8mol / L nitric acid solution. Then take 100mL of 8mol / L nitric acid solution and mix it with 10g of 400-mesh activated carbon after screening, and stir it at 80℃ and 300rpm for 8h. After stirring, filter the liquid and dry it to obtain Ac-HNO3.

[0071] The second step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0072] In the third step, 0.78 g of the catalyst carrier Ac-HNO3 is mixed with the ruthenium trichloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-HNO3.

[0073] The fourth step is to reduce 2.5wt%RuCl3 / Ac-HNO3 with sodium borohydride to obtain 2.5wt%Ru / Ac-HNO3. First, 0.325g of 2.5wt%RuCl3 / Ac-HNO3 is added to 40mL of water and stirred. Then 0.014g of sodium borohydride is mixed with 20mL of water. Then, the sodium borohydride aqueous solution is slowly added dropwise to the 2.5wt%RuCl3 / Ac-HNO3-melamine suspension within 10 minutes. The obtained liquid is filtered, and the obtained solid is dried to obtain the 2.5wt%Ru / Ac-HNO3 catalyst.

[0074] We use a two-step reaction method:

[0075] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), and 0.3047 g of chitin was added, and the mixture was placed in a reactor and reacted at 100°C and 0.5 MPa of nitrogen for 2 hours.

[0076] After cooling, add 0.1 g of 2.5 wt% Ru / Ac-HNO3-melamine catalyst, put it into the reactor again, and react for 2 hours at 250° C. and 3.0 MPa of hydrogen to obtain organic amine.

[0077] Example 7

[0078] There are four steps to prepare 2.5wt%Ru / Ac-melamine catalyst:

[0079] In the first step, 1.5 g of Ac and 1.5 g of melamine are mixed and ground and then put into a porcelain boat, and the porcelain boat containing the mixture is placed in a tube furnace, and nitrogen is passed through for 10 minutes, and then the temperature is raised from 25°C to 600°C over 190 minutes, and then maintained at 600°C for 120 minutes. After cooling, the catalyst carrier Ac-melamine can be obtained.

[0080] The second step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0081] In the third step, 0.78 g of the catalyst carrier Ac-melamine is mixed with the ruthenium chloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-melamine.

[0082] The fourth step is to reduce 2.5wt% RuCl3 / Ac-melamine with sodium borohydride to obtain 2.5wt% Ru / Ac-melamine. First, 0.325g of 2.5wt% RuCl3 / Ac-melamine is added to 40mL of water and stirred. Then 0.014g of sodium borohydride is mixed with 20mL of water. Then, the sodium borohydride aqueous solution is slowly added dropwise to the 2.5wt% RuCl3 / Ac-melamine suspension within 10 minutes. The obtained liquid is filtered, and the obtained solid is dried to obtain the 2.5wt% Ru / Ac-melamine catalyst.

[0083] We use a two-step reaction method:

[0084] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), and 0.3047 g of chitin was added, and the mixture was placed in a reactor and reacted at 100°C and 0.5 MPa of nitrogen for 2 hours.

[0085] After cooling, 0.1 g of 2.5 wt% Ru / Ac-melamine catalyst was added, and the mixture was put into the reactor again. The organic amine was obtained by reacting the mixture at 250° C. and 3.0 MPa of hydrogen for 2 hours.

[0086] Example 8

[0087] There are five steps to prepare 2.5wt%Ru / Ac-HNO3-melamine catalyst:

[0088] The first step is to make Ac-HNO3. First, mix 33.38mL of concentrated nitric acid with 66mL of water to obtain 8mol / L nitric acid solution. Then take 100mL of 8mol / L nitric acid solution and mix it with 10g of 400-mesh activated carbon after screening, and stir it at 80℃ and 300rpm for 8h. After stirring, filter the liquid and dry it to obtain Ac-HNO3.

[0089] In the second step, 1.5 g of Ac-HNO3 and 1.5 g of melamine were mixed and ground and then put into a porcelain boat, and the porcelain boat containing the mixture was placed in a tube furnace, and nitrogen was first passed for 10 minutes, and then the temperature was raised from 25°C to 600°C over 190 minutes, and then maintained at 600°C for 120 minutes. After cooling, the catalyst carrier Ac-HNO3-melamine was obtained.

[0090] The third step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0091] In the fourth step, 0.78 g of the catalyst carrier Ac-HNO3-melamine is mixed with the ruthenium trichloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is dried, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-HNO3-melamine.

[0092] The fifth step is to reduce 2.5wt%RuCl3 / Ac-HNO3-melamine with sodium borohydride to obtain 2.5wt%Ru / Ac-HNO3-melamine. First, 0.325g of 2.5wt%RuCl3 / Ac-HNO3-melamine is added to 40mL of water and stirred. Then 0.014g of NaOH is mixed with 20mL of water. Then, an aqueous sodium hydroxide solution is slowly added dropwise to the 2.5wt%RuCl3 / Ac-HNO3-melamine suspension within 10 minutes. The obtained liquid is filtered, and the obtained solid is dried to obtain a 2.5wt%Ru / Ac-HNO3-melamine catalyst.

[0093] We use a two-step reaction method:

[0094] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), and 0.3047 g of chitin was added, and the mixture was placed in a reactor and reacted at 100°C and 0.5 MPa of nitrogen for 2 hours.

[0095] After cooling, add 0.1 g of 2.5 wt% Ru / Ac-HNO3-melamine catalyst, put it into the reactor again, and react for 2 hours at 250° C. and 3.0 MPa of hydrogen to obtain organic amine.

[0096] The types of organic amines obtained in Examples 1-8 and the corresponding yields are as follows: Figure 1 shown.

[0097] Example 9

[0098] Preparation of 2.5wt%RuO x / Ac catalyst requires three steps:

[0099] The first step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0100] In the second step, 0.78 g of the catalyst carrier Ac-HNO3 is mixed with the ruthenium trichloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac.

[0101] In the third step, 2.5 wt% RuCl3 / Ac was hydrolyzed by sodium hydroxide (NaOH) to obtain 2.5 wt% RuO x / Ac. First, take 0.325g of 2.5wt% RuCl3 / Ac and add it to 40mL of water and stir. Then take 0.014g of NaOH and mix it with 20mL of water. Then slowly add the sodium hydroxide aqueous solution to the 2.5wt% RuCl3 / Ac suspension within 10min. Filter the obtained liquid and dry the obtained solid to obtain 2.5wt% RuO x / Ac catalyst.

[0102] For the reaction part, we use a one-step method:

[0103] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), 0.3047 g of chitin was added, and then 0.1 g of 2.5% wt RuO x / Ac catalyst, react at 250℃, 3.0MPa hydrogen for 2 hours to obtain organic amine.

[0104] Example 10

[0105] There are four steps to prepare 2.5wt% RuOx / Ac-HNO3 catalyst:

[0106] The first step is to make Ac-HNO3. First, mix 33.38mL of concentrated nitric acid with 66mL of water to obtain 8mol / L nitric acid solution. Then take 100mL of 8mol / L nitric acid solution and mix it with 10g of 400-mesh activated carbon after screening, and stir it at 80℃ and 300rpm for 8h. After stirring, filter the liquid and dry it to obtain Ac-HNO3.

[0107] The second step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0108] In the third step, 0.78 g of the catalyst carrier Ac-HNO3 is mixed with the ruthenium trichloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-HNO3.

[0109] The fourth step is to hydrolyze 2.5 wt% RuCl3 / Ac-HNO3 with sodium hydroxide (NaOH) to obtain 2.5 wt% RuO x / Ac-HNO3. First, take 0.325g of 2.5wt% RuCl3 / Ac-HNO3 and add it to 40mL of water and stir. Then take 0.014g of NaOH and mix it with 20mL of water. Then slowly add the sodium hydroxide aqueous solution to the 2.5wt% RuCl3 / Ac-HNO3-melamine suspension within 10min. Filter the obtained liquid, and then dry the obtained solid to obtain 2.5wt% RuO x / Ac-HNO3 catalyst.

[0110] For the reaction part, we use a one-step method:

[0111] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), 0.3047 g of chitin was added, and then 0.1 g of 2.5% wt RuO x / Ac-HNO3 catalyst, react at 250℃, 3.0MPa hydrogen conditions for 2 hours to obtain organic amine.

[0112] Embodiment 11

[0113] Preparation of 2.5wt%RuO x / Ac-melamine catalyst requires four steps:

[0114] In the first step, 1.5 g of Ac and 1.5 g of melamine are mixed and ground and then put into a porcelain boat, and the porcelain boat containing the mixture is placed in a tube furnace, and nitrogen is passed through for 10 minutes, and then the temperature is raised from 25°C to 600°C over 190 minutes, and then maintained at 600°C for 120 minutes. After cooling, the catalyst carrier Ac-melamine can be obtained.

[0115] The second step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0116] In the third step, 0.78 g of the catalyst carrier Ac-melamine is mixed with the ruthenium chloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-melamine.

[0117] The fourth step is to hydrolyze 2.5 wt% RuCl3 / Ac-melamine with sodium hydroxide (NaOH) to obtain 2.5 wt% RuO x / Ac-melamine. First, take 0.325g of 2.5wt% RuCl3 / Ac-melamine and add it to 40mL of water and stir. Then take 0.014g of NaOH and mix it with 20mL of water. Then slowly add the sodium hydroxide aqueous solution to the 2.5wt% RuCl3 / Ac-melamine suspension within 10min. Filter the obtained liquid, and then dry the obtained solid to obtain 2.5wt% RuO x / Ac-melamine catalyst.

[0118] For the reaction part, we use a one-step method:

[0119] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), 0.3047 g of chitin was added, and then 0.1 g of 2.5% wt RuO x / Ac-melamine catalyst, react at 250℃, 3.0MPa hydrogen for 2 hours to obtain organic amine.

[0120] Example 12

[0121] Preparation of 2.5wt%RuO x / Ac-HNO3-melamine catalyst requires five steps:

[0122] The first step is to make Ac-HNO3. First, mix 33.38mL of concentrated nitric acid with 66mL of water to obtain 8mol / L nitric acid solution. Then take 100mL of 8mol / L nitric acid solution and mix it with 10g of 400-mesh activated carbon after screening, and stir it at 80℃ and 300rpm for 8h. After stirring, filter the liquid and dry it to obtain Ac-HNO3.

[0123] In the second step, 1.5 g of Ac-HNO3 and 1.5 g of melamine were mixed and ground and then put into a porcelain boat, and the porcelain boat containing the mixture was placed in a tube furnace, and nitrogen was first passed for 10 minutes, and then the temperature was raised from 25°C to 600°C over 190 minutes, and then maintained at 600°C for 120 minutes. After cooling, the catalyst carrier Ac-HNO3-melamine was obtained.

[0124] The third step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0125] In the fourth step, 0.78 g of the catalyst carrier Ac-HNO3-melamine is mixed with the ruthenium trichloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is dried, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-HNO3-melamine.

[0126] The fifth step is to hydrolyze 2.5wt%RuCl3 / Ac-HNO3-melamine with sodium hydroxide (NaOH) to obtain 2.5wt%RuO x / Ac-HNO3-melamine. First, take 0.325g of 2.5wt% RuCl3 / Ac-HNO3-melamine and add it to 40mL of water and stir. Then take 0.014g of NaOH and mix it with 20mL of water. Then slowly add the sodium hydroxide aqueous solution to the 2.5wt% RuCl3 / Ac-HNO3-melamine suspension within 10min. Filter the obtained liquid, and then dry the obtained solid to obtain 2.5wt% RuO x / Ac-HNO3-melamine catalyst.

[0127] For the reaction part, we use a one-step method:

[0128] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), 0.3047 g of chitin was added, and then 0.1 g of 2.5% wt RuO x / Ac-HNO3-melamine catalyst, react at 250℃, 3.0MPa hydrogen conditions for 2 hours to obtain organic amine.

[0129] Example 13

[0130] There are three steps to prepare 2.5wt%Ru / Ac catalyst:

[0131] The first step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0132] In the second step, 0.78 g of the catalyst carrier Ac-HNO3 is mixed with the ruthenium trichloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac.

[0133] In the third step, 2.5 wt% RuCl3 / Ac was reduced by sodium borohydride to obtain 2.5 wt% RuO x / Ac. First, take 0.325g of 2.5wt% RuCl3 / Ac and add it to 40mL of water and stir. Then take 0.014g of sodium borohydride and mix it with 20mL of water. Then slowly add the sodium borohydride aqueous solution to the 2.5wt% RuCl3 / Ac suspension within 10min. Filter the obtained liquid, and then dry the obtained solid to obtain a 2.5wt% Ru / Ac catalyst.

[0134] For the reaction part, we use a one-step method:

[0135] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), 0.3047 g of chitin was added, and then 0.1 g of 2.5% wt Ru / Ac catalyst was added, and the reaction was carried out at 250° C. and 3.0 MPa of hydrogen for 2 hours to obtain an organic amine.

[0136] Embodiment 14

[0137] There are four steps to prepare 2.5wt%Ru / Ac-HNO3 catalyst:

[0138] The first step is to make Ac-HNO3. First, mix 33.38mL of concentrated nitric acid with 66mL of water to obtain 8mol / L nitric acid solution. Then take 100mL of 8mol / L nitric acid solution and mix it with 10g of 400-mesh activated carbon after screening, and stir it at 80℃ and 300rpm for 8h. After stirring, filter the liquid and dry it to obtain Ac-HNO3.

[0139] The second step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0140] In the third step, 0.78 g of the catalyst carrier Ac-HNO3 is mixed with the ruthenium trichloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-HNO3.

[0141] The fourth step is to reduce 2.5wt%RuCl3 / Ac-HNO3 by sodium borohydride to obtain 2.5wt%RuO x / Ac-HNO3. First, take 0.325g of 2.5wt% RuCl3 / Ac-HNO3 and add it to 40mL of water and stir. Then take 0.014g of sodium borohydride and mix it with 20mL of water. Then, slowly add the sodium borohydride aqueous solution to the 2.5wt% RuCl3 / Ac-HNO3-melamine suspension within 10 minutes. Filter the obtained liquid, and then dry the obtained solid to obtain a 2.5wt% Ru / Ac-HNO3 catalyst.

[0142] For the reaction part, we use a one-step method:

[0143] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), 0.3047 g of chitin was added, and then 0.1 g of 2.5% wt Ru / Ac-HNO3 catalyst was added. The organic amine was obtained by reacting at 250°C and 3.0 MPa of hydrogen for 2 hours.

[0144] Embodiment 15

[0145] There are four steps to prepare 2.5wt%Ru / Ac-melamine catalyst:

[0146] In the first step, 1.5 g of Ac and 1.5 g of melamine are mixed and ground and then put into a porcelain boat, and the porcelain boat containing the mixture is placed in a tube furnace, and nitrogen is passed through for 10 minutes, and then the temperature is raised from 25°C to 600°C over 190 minutes, and then maintained at 600°C for 120 minutes. After cooling, the catalyst carrier Ac-melamine can be obtained.

[0147] The second step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0148] In the third step, 0.78 g of the catalyst carrier Ac-melamine is mixed with the ruthenium chloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is stirred dry, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-melamine.

[0149] The fourth step is to reduce 2.5wt% RuCl3 / Ac-melamine with sodium borohydride to obtain 2.5wt% Ru / Ac-melamine. First, 0.325g of 2.5wt% RuCl3 / Ac-melamine is added to 40mL of water and stirred. Then 0.014g of sodium borohydride is mixed with 20mL of water. Then, the sodium borohydride aqueous solution is slowly added dropwise to the 2.5wt% RuCl3 / Ac-melamine suspension within 10 minutes. The obtained liquid is filtered, and the obtained solid is dried to obtain the 2.5wt% Ru / Ac-melamine catalyst.

[0150] For the reaction part, we use a one-step method:

[0151] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), 0.3047 g of chitin was added, and then 0.1 g of 2.5% wt Ru / Ac-melamine catalyst was added. The organic amine was obtained by reacting at 250° C. and 3.0 MPa of hydrogen for 2 hours.

[0152] Example 16

[0153] There are five steps to prepare 2.5wt%Ru / Ac-HNO3-melamine catalyst:

[0154] The first step is to make Ac-HNO3. First, mix 33.38mL of concentrated nitric acid with 66mL of water to obtain 8mol / L nitric acid solution. Then take 100mL of 8mol / L nitric acid solution and mix it with 10g of 400-mesh activated carbon after screening, and stir it at 80℃ and 300rpm for 8h. After stirring, filter the liquid and dry it to obtain Ac-HNO3.

[0155] In the second step, 1.5 g of Ac-HNO3 and 1.5 g of melamine were mixed and ground and then put into a porcelain boat, and the porcelain boat containing the mixture was placed in a tube furnace, and nitrogen was first passed for 10 minutes, and then the temperature was raised from 25°C to 600°C over 190 minutes, and then maintained at 600°C for 120 minutes. After cooling, the catalyst carrier Ac-HNO3-melamine was obtained.

[0156] The third step is to prepare a ruthenium chloride (RuCl3) acetone solution. 0.041 g of RuCl3 was mixed with 15 mL of acetone and stirred at 300 rpm for 6 h.

[0157] In the fourth step, 0.78 g of the catalyst carrier Ac-HNO3-melamine is mixed with the ruthenium trichloride (RuCl3) acetone solution obtained in the third step, and stirring is continued in a fume hood until the liquid is dried, and then drying is performed to obtain 2.5 wt% RuCl3 / Ac-HNO3-melamine.

[0158] The fifth step is to reduce 2.5wt%RuCl3 / Ac-HNO3-melamine with sodium borohydride to obtain 2.5wt%Ru / Ac-HNO3-melamine. First, 0.325g of 2.5wt%RuCl3 / Ac-HNO3-melamine is added to 40mL of water and stirred. Then 0.014g of sodium borohydride is mixed with 20mL of water. Then, the sodium borohydride aqueous solution is slowly added dropwise to the 2.5wt%RuCl3 / Ac-HNO3-melamine suspension within 10 minutes. The obtained liquid is filtered, and the obtained solid is dried to obtain the 2.5wt%Ru / Ac-HNO3-melamine catalyst.

[0159] For the reaction part, we use a one-step method:

[0160] First, 15 mL of water was mixed with 0.86465 g of phosphoric acid (H3PO4), 0.3047 g of chitin was added, and then 0.1 g of 2.5% wt Ru / Ac-HNO3-melamine catalyst was added. The organic amine was obtained by reacting at 250°C and 3.0 MPa of hydrogen for 2 hours.

[0161] The types of organic amines obtained in Examples 9-16 and the corresponding yields are as follows: Figure 2 shown.

Claims

1. A method for preparing bio-based amine compounds by two-step conversion of marine biomass, characterized in that: The following steps are involved: 1) Mix 30% to 68% nitric acid aqueous solution with 0.05 to 0.25 mass equivalent of activated carbon, i.e. Ac, and stir at 60 to 100° C. and 100 to 1000 rpm for 1 to 24 hours to obtain Ac-HNO3; Mix Ac-HNO3 and melamine in a mass ratio of 1:1 to 1:5, grind them, place them in a tube furnace, and flow a nitrogen gas flow rate of 0.1 to 200 mL / min, then heat the mixture from 25° C. to 400 to 600° C., keep it for 120 to 360 minutes, and cool it down to obtain the catalyst carrier Ac-HNO3-melamine; Mix Ac and melamine, i.e. melamine, in a mass ratio of 1:1 to 1:5, grind them, place them in a tube furnace, and flow a nitrogen gas flow rate of 0.1 to 200 mL / min, then heat the mixture from 25° C. to 400 to 800° C., keep it for 0 .5~10h, after cooling, the catalyst carrier Ac-melamine can be obtained; RuCl3 is dissolved in acetone, and mixed with the catalyst carrier Ac, AC-HNO3, Ac-melamine, Ac-HNO3-melamine at a Ru mass loading rate of 0.5%~10%, respectively, and stirred until the liquid is dried to obtain RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, RuCl3 / Ac-HNO3-melamine respectively; RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, RuCl3 / Ac-HNO3-melamine are hydrolyzed with sodium hydroxide equivalent to 1~10 times the mass of Ru to obtain RuO x / Ac、RuO x / Ac-HNO3、RuO x / Ac-melamine、RuO x / Ac-HNO3-melamine; RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, RuCl3 / Ac-HNO3-melamine were reduced by sodium borohydride equivalent to 0.1 to 100 times the mass of Ru to obtain Ru / Ac, Ru / Ac-HNO3, Ru / Ac-melamine, Ru / Ac-HNO3-melamine respectively; 2) Mix 75-95% water, 1-30% phosphoric acid and 0.5-30% chitin, place in a reaction kettle, and react for 1-8 hours at 80-150° C. and 0.1-10 MPa nitrogen; 3) After the reaction liquid is cooled, one or more catalysts equivalent to 0.1-10% of the above reaction liquid are added, and the mixture is put into the reactor again to react for 1-10 hours at 200-250° C. and 1.0-3.0 MPa of hydrogen to obtain a phosphorylated organic amine.

2. A method for preparing bio-based amine compounds by one-step conversion of marine biomass, characterized in that: The following steps are involved: 1) Mix 30% to 68% nitric acid aqueous solution with 0.05 to 0.25 mass equivalent of activated carbon, i.e. Ac, and stir at 60 to 100° C. and 100 to 1000 rpm for 1 to 24 hours to obtain Ac-HNO3; Mix Ac-HNO3 and melamine in a mass ratio of 1:1 to 1:5, grind them, place them in a tube furnace, and flow a nitrogen gas flow rate of 0.1 to 200 mL / min, then heat the mixture from 25° C. to 400 to 600° C., keep it for 120 to 360 minutes, and cool it down to obtain the catalyst carrier Ac-HNO3-melamine; Mix Ac and melamine, i.e. melamine, in a mass ratio of 1:1 to 1:5, grind them, place them in a tube furnace, and flow a nitrogen gas flow rate of 0.1 to 200 mL / min, then heat the mixture from 25° C. to 400 to 800° C., keep it for 0 .5~10h, after cooling, the catalyst carrier Ac-melamine can be obtained; RuCl3 is dissolved in acetone, and mixed with the catalyst carrier Ac, AC-HNO3, Ac-melamine, Ac-HNO3-melamine at a Ru mass loading rate of 0.5%~10%, respectively, and stirred until the liquid is dried to obtain RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, RuCl3 / Ac-HNO3-melamine respectively; RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, RuCl3 / Ac-HNO3-melamine are hydrolyzed with sodium hydroxide equivalent to 1~10 times the mass of Ru to obtain RuO x / Ac、RuO x / Ac-HNO3、RuO x / Ac-melamine、RuO x / Ac-HNO3-melamine; RuCl3 / Ac, RuCl3 / Ac-HNO3, RuCl3 / Ac-melamine, RuCl3 / Ac-HNO3-melamine were reduced by sodium borohydride equivalent to 0.1 to 100 times the mass of Ru to obtain Ru / Ac, Ru / Ac-HNO3, Ru / Ac-melamine, Ru / Ac-HNO3-melamine respectively; 2) 75-95% water, 1-30% phosphoric acid, 0.5-30% chitin, and 0.1-10% of one or more of the above catalysts are mixed, placed in a reaction kettle, and reacted for 1-10 hours at 200-250° C. and 1.0-3.0 MPa hydrogen to obtain a phosphorylated organic amine.

3. The method according to claim 1-2, characterized in that: The mass ratio of Ac-HNO3 to melamine is 1:5 to 5:1, and the temperature of the tubular furnace is increased from 30°C to 600°C and maintained for 2 hours.

4. An organic amine prepared according to the method of claims 1-2, characterized in that: The organic amines include linear amines and cyclic amines, wherein the linear amines are one or more of ethylamine, propylamine and butylamine, and the cyclic amines are one or more of pyrrolidine, 2-methylpyrrolidine, 2,5-dimethylpyrrolidine, piperidine and 2-methylpiperidine. The yield of the organic amines is 5-99%.

Citation Information

Patent Citations

  • Mixed ruthenium base amino synthetic catalyst and its preparing method

    CN1820843A

  • Hydrogenation using chitin and chitosan based immobilized metal catalysts

    US4431836A

  • Method for synthesizing amines

    WO2008138833A1