A glass fiber reinforced plastic plate, a composite plate and a preparation method and application thereof

By setting up concave and convex patterns on the fiberglass sheet and using chain agent, combined with the assembly line continuous mechanism, the problems of poor bonding effect and low production efficiency of fiberglass panels in the polyurethane foaming integrated composite process are solved, and efficient and stable composite boards are achieved Production and excellent mechanical properties.

CN117621567BActive Publication Date: 2024-11-26SHANDONG YUANSHI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311691989.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-11
Publication Date
2024-11-26
Estimated Expiration
2043-12-11

AI Technical Summary

Technical Problem

In the integrated polyurethane foaming composite process, the bonding effect between the fiberglass panel and the polyurethane foaming material is poor, resulting in serious quality defects such as bulging and delamination. In addition, the traditional fiberglass panel production process has problems such as unstable quality and low production efficiency.

Method used

Design of fiberglass sheets combining the matrix layer and the surface resin layer, with concave and convex patterns on the surface resin layer, and chain agent is added to the matrix layer to improve bonding strength and fluidity, and molding at one time through the continuous assembly line mechanism to avoid joints. The problem of cumbersome construction and low efficiency.

Benefits of technology

It significantly improves the bonding effect between fiberglass sheet and polyurethane foaming material, avoids quality defects such as bulging and delamination, improves production efficiency and mechanical properties, and reduces the weight and energy consumption of composite sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117621567B_ABST
    Figure CN117621567B_ABST
Patent Text Reader

Abstract

The present invention relates to a glass fiber reinforced plastic sheet, a composite plate and a preparation method and application thereof, and relates to the field of glass fiber reinforced plastic composite plates, comprising a base layer and a surface resin layer, wherein a surface resin layer is provided on one side of the base layer, and a concave-convex pattern is provided on the surface resin layer, and the base layer comprises the following raw materials in parts by weight: 1-5 parts of a continuous reinforcement layer, 1-153 parts of an unsaturated polyester resin A5, 1-3 parts of a curing agent A, 0.11-0.33 parts of an initiator A, and 0.06-0.18 parts of an inhibitor A; the surface resin layer comprises the following raw materials in parts by weight: 1.35-9.6 parts of a chain agent. The present invention avoids the problem of serious quality defects such as bulging and delamination caused by poor bonding effect between the bonding surface of the glass fiber reinforced plastic panel and the polyurethane foam material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of glass fiber reinforced plastic composite plates, and in particular to a glass fiber reinforced plastic plate, a composite plate, and a preparation method and application thereof. Background Art

[0002] Polyurethane sandwich fiberglass composite panel refers to a composite panel using fiberglass as the panel and polyurethane foam as the sandwich panel. The traditional composite process of polyurethane sandwich fiberglass composite panel is to use fiberglass panel and polyurethane foam sandwich, and bond them by applying glue. The gaps between the foams need to be manually spliced ​​with glue and glass fiber materials, and the facades around the composite panel also need to be manually wrapped with glue and glass fiber materials. Due to the large amount of glue and glass fiber used, the sandwich composite panel is very heavy, such as patent CN 113276528 A-A refrigeration insulation composite panel and its processing technology.

[0003] At present, the polyurethane foam integrated composite process directly injects polyurethane foam into the cavity formed by the fiberglass panel and the surrounding fixtures, maintains pressure, and then completes the composite. This process is not only efficient, but also does not require the use of glue. The internal polyurethane is directly bonded to the panel after foaming, and there is no seam. The composite panel facade does not need to be edge-sealed. The integrated composite makes the cold bridge problem, thermal insulation performance, structural strength and weight highly optimized, making it more energy-saving and environmentally friendly.

[0004] However, the polyurethane foam integrated composite process has serious bottleneck constraints, mainly because the bonding effect between the FRP panel bonding surface and the polyurethane foam material is not good, which easily causes serious quality defects such as bulging and delamination, thus preventing the composite process from being widely promoted and applied. In addition, the production processes of FRP panels include manual mold board making, discontinuous machine board making and continuous machine board making. The production processes of manual mold board making and discontinuous machine board making have a series of problems such as unstable quality and low production efficiency. The composite materials cannot play the maximum efficiency, resulting in waste of resources, which results in high cost of FRP panels, affecting the promotion and application of FRP panels.

[0005] At present, the methods for solving the adhesion of the bonding surface of FRP panels mainly include corona and grinding processes. For the polyurethane foam integrated composite process, the corona process has poor effect, while the grinding process has relatively good effect. However, the grinding process has the problems of unstable effect, large dust, easy damage to the microscopic bonding surface, and material wear and waste. Polyurethane foam materials are afraid of dust, and dust removal after grinding is very demanding. In view of this, the present invention provides a FRP plate, a composite plate, and a preparation method and application thereof. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a glass fiber reinforced plastic sheet, a composite board and a preparation method and application thereof. The purpose is to provide a glass fiber reinforced plastic sheet for a polyurethane foam integrated composite process and a prepared composite board, so as to avoid the problem of serious quality defects such as bulging and delamination caused by poor bonding effect between the bonding surface of the glass fiber reinforced plastic panel and the polyurethane foam material.

[0007] In order to solve the above technical problems, the first aspect of the present invention is to provide a glass fiber reinforced plastic plate material, including a base layer and a surface resin layer, wherein the surface resin layer is provided on one side of the base layer, and the surface resin layer is provided with a concave-convex pattern, and the base layer comprises the following raw materials in parts by weight: 1-5 parts of continuous reinforcement layer, 1-153 parts of unsaturated polyester resin A5, 1-3 parts of curing agent A, 0.11-0.33 parts of initiator A, and 0.06-0.18 parts of inhibitor A; the surface resin layer comprises the following raw materials in parts by weight: 1.35-9.6 parts of chain agent.

[0008] The beneficial effects of the present invention are:

[0009] (1) The fiberglass sheet of the present invention is an integral flat plate, and a concave-convex pattern (e.g., an inward-facing patterned pockmarked surface) is formed on one side of the base layer, so that the entire fiberglass sheet has a friendly bonding interface; when it is applied to downstream products of the fiberglass panel, such as a polyurethane foaming integrated composite process, on the one hand, the polyurethane foam material and the base layer can be integrated, the contact area between the base layer and the polyurethane foam material is increased, and the polyurethane foam material enters the interior of the concave-convex pattern to produce a vertical structure, thereby improving the bonding between the two and largely avoiding the problem of serious quality defects such as bulging and delamination; on the other hand, the concave-convex pattern of the base layer of the present invention improves the fluidity of the foaming process and increases the foaming rate of the bonding surface with the polyurethane foam material, thereby deeply compounding the fiberglass sheet and the polyurethane foam; thereby improving the poor bonding effect of the existing foaming composite process and serious quality defects such as bulging and delamination;

[0010] (2) Chain-building agents are substances that can react with functional groups on linear polymer chains to extend the molecular chains and increase the molecular weight. They are used to improve the mechanical properties and process properties of products such as polyurethanes and polyesters. In production, some compounds containing active hydrogen react with isocyanate-terminated prepolymers to cause the molecular chains to diffuse and extend, thereby achieving the curing and forming of the resin. In the polyester processing technology, the molecular weight decreases due to thermal degradation and hydrolysis, and the number of terminal carboxyl groups increases, thereby reducing the mechanical and chemical properties of the polymer. Add difunctional small molecule compounds under reactive blending conditions. For example: difunctional acid derivatives, isocyanates, anhydrides and epoxides, etc. These difunctional compounds contain functional groups that are easily reactive with carboxyl, hydroxyl and amino groups, and can directly react with low molecular weight oligomers to form a "bridge" between the two polymer chains, significantly increasing the molecular weight, increasing the viscosity of the system, and reducing the terminal carboxyl content. The ends of linear polyesters mainly include hydroxyl and carboxyl groups, so chain extension of polyesters is to select compounds to add to hydroxyl or carboxyl groups.

[0011] Based on the above technical solution, the present invention can also be improved as follows.

[0012] Furthermore, the base layer includes the following raw materials in parts by weight: 3 parts of continuous reinforcement layer, 102 parts of unsaturated polyester resin A, 2 parts of curing agent A, 0.22 parts of initiator A, and 0.12 parts of inhibitor A.

[0013] Further, the continuous reinforcement layer comprises any one of surface felt, glass fiber chopped yarn, chopped strand mat, woven cloth, glass fiber felt, glass fiber cloth, carbon fiber, basalt fiber, multi-axial cloth, stitched felt, and warp knitted cloth, or a combination of at least two of them. When a combination of at least two is used, the weight ratio of each component is any ratio; the unsaturated polyester resin A comprises isophthalic unsaturated polyester resin; the curing agent A comprises methyl ethyl ketone peroxide; the initiator A comprises a cobalt-based initiator; the inhibitor A comprises DPPH (1,1-diphenyl-2 -trinitrophenylhydrazine), TBC (inhibitor TBC), phenol, ferric chloride, any one or a combination of at least two thereof; the chain-building agent includes ethylene glycol, propylene glycol, 1,4-butanediol, diethylene glycol, glycerol, trimethylolpropane, 1,4-cyclohexanediol, hydrogenated bisphenol A, dimethylene phenyl glycol, hydroquinone bis-β-hydroxyethyl ether, resorcinol hydroxy ether, diethanolamine, triethanolamine, methyldiethanolamine, diethyltoluenediamine, 3,5-dimethylthiotoluenediamine, any one or a combination of at least two thereof;

[0014] The depth of the concave-convex pattern is 300-500um.

[0015] The beneficial effect of adopting the above further scheme is: the present invention adopts any one of surface felt, glass fiber chopped yarn, chopped mat, woven cloth, glass fiber felt, glass fiber cloth, carbon fiber, basalt fiber, multi-axial cloth, stitched felt, and warp knitted cloth, or a combination of at least two of them as a continuous reinforcement layer, so that the fiber content of the glass fiber reinforced plastic sheet is high, and it has excellent mechanical properties, shear properties, high tensile strength, and good impact resistance. The Barcol hardness of the prepared glass fiber reinforced plastic sheet reaches more than 45HBa, which has good practical value for the glass fiber reinforced plastic panel.

[0016] Furthermore, the base layer further comprises 6.68-20.04 parts of a skeleton material; the skeleton material comprises any one or a combination of at least two of aluminum hydroxide, diatomaceous earth, talc, kaolin, hollow microspheres, cellulose, ceramic powder, mica, and pearl powder. When a combination of at least two is used, the weight ratio of each component is any ratio. Preferably, the base layer further comprises 6.68 parts, 13.36 parts, 20.04 parts, etc. of the skeleton material.

[0017] The beneficial effect of adopting the above further scheme is: the present invention makes the board lighter by adopting a skeleton material, thereby reducing the weight of the board while ensuring the hardness, so that after using polyurethane foam composite, the weight of the entire composite board is reduced, energy consumption is reduced, and it is more widely used. Further, the FRP sheet material further comprises a gel coat layer, which is arranged on the other side of the base layer, and the gel coat layer comprises the following raw materials in parts by weight: 53-159 parts of unsaturated polyester resin B, 4.9-14.7 parts of flexible unsaturated resin, 1-3 parts of curing agent B, 0.45-1.35 parts of initiator B, 0.67-2.01 parts of defoamer, 0.63-1.89 parts of leveling agent, and 0.185-0.555 parts of inhibitor B; preferably, the gel coat layer comprises the following raw materials in parts by weight: 106 parts of unsaturated polyester resin B, 9.8 parts of flexible unsaturated resin, 2 parts of curing agent B, 0.9 parts of initiator B, 1.34 parts of defoamer, 1.26 parts of leveling agent, and 0.37 parts of inhibitor B;

[0018] The unsaturated polyester resin B includes isophthalic unsaturated polyester resin, and the flexible unsaturated resin includes orthophthalic unsaturated polyester resin; the curing agent B includes methyl ethyl ketone peroxide; the initiator B includes a cobalt-based initiator; the defoamer includes a polysiloxane carbon-based compound or a GPES polyether defoamer; the leveling agent includes a modified polysiloxane compound; the inhibitor B includes any one of DPPH, TBC, phenol, and ferric chloride, or a combination of at least two thereof;

[0019] The outer surface of the gel coat layer is provided with concave-convex patterns with a depth of 50±10 um.

[0020] The beneficial effect of adopting the above further scheme is: the gel coat layer of the present invention adopts a combination of unsaturated polyester resin and flexible unsaturated resin, so that the fiberglass panel has better toughness and weather resistance; at the same time, the outer surface of the gel coat layer is provided with a concave-convex pattern with a depth of 50±10um, similar to shark skin, which can make the fiberglass panel have less air resistance when moving.

[0021] The second aspect of the present invention is to provide a method for preparing the glass fiber reinforced plastic sheet as described above, comprising the following steps:

[0022] (1) unsaturated polyester resin A, curing agent A, initiator A and inhibitor A are mixed to obtain a matrix raw material mixed liquid, and the matrix raw material mixed liquid is applied layer by layer to infiltrate the continuous reinforcement layer to obtain a glass fiber reinforced plastic sheet precursor;

[0023] (2) firstly coating one side of the glass fiber reinforced plastic sheet precursor with an unsaturated polyester resin C, wherein the unsaturated polyester resin C includes a chain-binding agent, to form a surface resin layer, and then bonding a concave-convex pattern film, and then sequentially performing roller pressing, heating curing and negative pressure heating to obtain a glass fiber reinforced plastic sheet with a concave-convex pattern;

[0024] Alternatively, unsaturated polyester resin C is first coated on one side of the FRP sheet precursor, wherein the unsaturated polyester resin C includes a chain-binding agent to form a surface resin layer, and then a base film is bonded thereto, and then the surface is passed through a patterned roller track, and finally rolling, heating and curing, and negative pressure heating are performed in sequence to obtain a FRP sheet with a concave-convex pattern.

[0025] The beneficial effects of adopting the above scheme are as follows: the fiberglass panel of the present invention is formed in one step by a continuous assembly line mechanism, without splicing and without joints, to obtain a continuous plate with an integrated structure, and a concave-convex pattern is obtained by bonding a concave-convex pattern film or by rolling with a patterned roller track to obtain a side surface of the base layer with a concave-convex pattern. It has high production efficiency, saves raw materials, avoids the problems of complicated joint construction, low efficiency, high cost, unsightly appearance and difficulty in waterproofing, improves the problems existing in the production process of manual mold plate making and non-continuous mechanism plate making, and can meet market demand.

[0026] Further, step (1) includes the following specific steps:

[0027] (1-1) Preparation of gel coat layer: unsaturated polyester resin B, flexible unsaturated resin, curing agent B, initiator B, defoamer, leveling agent, and inhibitor B are mixed to obtain gel coat layer raw material liquid, the gel coat layer raw material liquid is sprayed onto the base film of gel coat layer, and heated and cured to obtain gel coat layer;

[0028] (1-2) Unsaturated polyester resin A, curing agent A, initiator A, inhibitor A and skeleton material are mixed to obtain a matrix raw material mixed liquid, and the matrix raw material mixed liquid is applied layer by layer on the surface of the gel coat layer to infiltrate the continuous reinforcement layer to obtain a glass fiber reinforced plastic sheet precursor containing a gel coat layer.

[0029] Furthermore, in step (2), the unsaturated polyester resin C further comprises isophthalic unsaturated polyester resin or vinyl resin. When a combination of the two is used, the weight ratio of each component is any ratio; the temperature for heating and curing is 80-135° C.; the temperature for negative pressure heating is 80° C. and the pressure is 15-40 KPa;

[0030] In step (1-1), the temperature for heating and curing is 80-135°C.

[0031] The heating curing of the present invention includes medium temperature curing and high temperature curing; the temperature of the medium temperature curing is 80-100°C, and the curing agent is V388 methyl ethyl ketone peroxide; preferably, the temperature of the medium temperature curing is 80-100°C, and the curing agent is M50 methyl ethyl ketone peroxide; the temperature of the high temperature curing is 105-140°C, and the curing agent is CHP (isopropylbenzene hydroperoxide).

[0032] The third aspect of the present invention is to provide a composite board, comprising the fiberglass reinforced plastic board as described above.

[0033] Furthermore, the composite board includes an upper surface layer, a lower surface layer and a core layer which are integrally formed, the core layer is arranged between the upper surface layer and the lower surface layer, the upper surface layer and the lower surface layer are both the fiberglass reinforced plastic sheet material, and the core layer is polyurethane foam.

[0034] The beneficial effects of adopting the above scheme are: the composite board of the present invention, that is, the polyurethane sandwich fiberglass composite board, is prepared by adopting a polyurethane foaming integrated composite process. Since no glue is used, it is environmentally friendly, non-toxic and odorless; and has the properties of high and low temperature resistance, corrosion resistance, and not easy to change color. The resin of the base layer is heated under negative pressure in the post-curing stage to discharge organic waste gas, so there is no irritating odor.

[0035] A fourth aspect of the present invention is to provide an application of the composite plate as described above, wherein the composite plate is used in cold chain logistics.

[0036] A fifth aspect of the present invention is to provide a method for preparing the composite board as described above, wherein the composite board is prepared by using a polyurethane foaming integrated composite process.

[0037] The composite board prepared by the polyurethane foaming integrated composite process does not require the use of glue or a composite surface adhesive layer, thereby improving the poor bonding effect of the existing foaming composite process, serious quality defects such as bulging and delamination, and adopts a continuous one-time molding process on an assembly line, has high production efficiency, saves raw materials, and can meet market demand. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic diagram of the structure of the composite plate of the present invention. DETAILED DESCRIPTION

[0039] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0040] The reagents and materials used in the following experimental examples and comparative examples are as follows:

[0041] Isophthalic unsaturated polyester resin: 972 resin from Jinan Yisheng Resin Co., Ltd.; cobalt-based initiator BZ-105 from Shanghai Yongyan Chemical Technology Co., Ltd.; orthophthalic unsaturated polyester resin: TC-191 resin from Wanqing Chemical Technology Co., Ltd.; polysiloxane carbon-based compound: GSK-5000 from Dongguan Gaosijin Fine Chemical Co., Ltd.; GPES polyether defoamer: DF-2692 from Dongguan Defeng Defoamer; modified polysiloxane compound: ByK-6333 from Dongguan Gaosijin Fine Chemical Co., Ltd.

[0042] Example 1

[0043] The present embodiment relates to a glass fiber reinforced plastic sheet material, comprising a base layer, a surface resin layer and a gel coat layer, wherein the surface resin layer is provided on one side of the base layer, and a concave-convex pattern is provided on the surface resin layer, and the gel coat layer is provided on the other side of the base layer, and the base layer comprises the following raw materials in parts by weight: 3 parts of continuous reinforcement layer, 102 parts of unsaturated polyester resin A, 2 parts of curing agent A, 0.22 parts of initiator A, 0.12 parts of inhibitor A, and 13.36 parts of skeleton material; the gel coat layer comprises the following raw materials in parts by weight: 106 parts of unsaturated polyester resin B, 9.8 parts of flexible unsaturated resin, 2 parts of curing agent B, 0.9 parts of initiator B, 1.34 parts of defoaming agent, 1.26 parts of leveling agent, and 0.37 parts of inhibitor B; the surface resin layer comprises the following raw materials in parts by weight: 6.5 parts of chain agent.

[0044] Preferably, the continuous reinforcement layer is any one of surface felt, glass fiber chopped yarn, chopped strand mat, woven cloth, glass fiber felt, glass fiber cloth, carbon fiber, basalt fiber, multi-axial cloth, stitched felt, and warp knitted cloth, or a combination of at least two of them.

[0045] Specifically, the continuous reinforcement layer is 1 part of glass fiber chopped yarn, 0.6 part of glass fiber mat, and 0.4 part of stitched mat; the unsaturated polyester resin A is isophthalic unsaturated polyester resin; the curing agent A is methyl ethyl ketone peroxide; the initiator A is a cobalt-based initiator; the inhibitor A is DPPH, TBC, phenol and ferric chloride, and the ratio of DPPH, TBC, phenol and ferric chloride is 1:1:1:1; the chain scissor is 6.54 parts. The chain scissor is methyl diethanolamine.

[0046] Wherein, the depth of the concave-convex pattern is 300-500um.

[0047] Preferably, the skeleton material is any one or a combination of at least two of aluminum hydroxide, diatomaceous earth, talc, kaolin, hollow microspheres, cellulose, ceramic powder, mica, and pearl powder. Specifically, 3.6 parts of cellulose, 2.66 parts of pearl powder, and 7.4 parts of mica.

[0048] Specifically, the unsaturated polyester resin B is an isophthalic unsaturated polyester resin, the flexible unsaturated resin is an orthophthalic unsaturated polyester resin; the curing agent B is methyl ethyl ketone peroxide; the initiator B is a cobalt-based initiator; the defoaming agent is a polysiloxane carbon-based compound or a GPES polyether defoaming agent; the leveling agent is a modified polysiloxane compound; the inhibitor B is DPPH, TBC, phenol, and ferric chloride, and the dosage ratio of DPPH, TBC, phenol and ferric chloride is 1:1:1:1.

[0049] Wherein, the outer surface of the gel coat layer is provided with concave-convex patterns with a depth of 50±10 um.

[0050] The present invention provides a method for preparing the glass fiber reinforced plastic sheet as described above, comprising the following steps:

[0051] (1) unsaturated polyester resin A, curing agent A, initiator A and inhibitor A are mixed to obtain a matrix raw material mixed liquid, and the matrix raw material mixed liquid is applied layer by layer to infiltrate the continuous reinforcement layer to obtain a glass fiber reinforced plastic sheet precursor;

[0052] Specifically, step (1) includes the following specific steps:

[0053] (1-1) Preparation of gel coat layer: unsaturated polyester resin B, flexible unsaturated resin, curing agent B, initiator B, defoamer, leveling agent, and inhibitor B are mixed to obtain gel coat layer raw material liquid, the gel coat layer raw material liquid is sprayed onto the base film of gel coat layer, and heated and cured to obtain gel coat layer;

[0054] (1-2) Unsaturated polyester resin A, curing agent A, initiator A, inhibitor A and skeleton material are mixed to obtain a matrix raw material mixed liquid, and the matrix raw material mixed liquid is applied layer by layer on the surface of the gel coat layer to infiltrate the continuous reinforcement layer to obtain a glass fiber reinforced plastic sheet precursor containing a gel coat layer.

[0055] (2) First, one side of the glass fiber reinforced plastic sheet precursor is coated with unsaturated polyester resin C, wherein the unsaturated polyester resin C includes a chain-binding agent to form a surface resin layer, and then a concave-convex pattern film is bonded thereto, and then rolling, heating and curing, and negative pressure heating are performed in sequence to obtain a glass fiber reinforced plastic sheet with a concave-convex pattern.

[0056] Specifically, in step (2), the unsaturated polyester resin C further comprises isophthalic unsaturated polyester resin and vinyl resin, and the weight ratio of the isophthalic unsaturated polyester resin to the vinyl resin is 0.2-0.5 Kg / m 2 ; The temperature for heating and curing is 80-135℃; the temperature for negative pressure heating is 80℃ and the pressure is 30KPa;

[0057] In step (1-1), the temperature for heating and curing is 80-135°C.

[0058] Example 2

[0059] The present embodiment relates to a glass fiber reinforced plastic sheet, comprising a base layer, a surface resin layer and a gel coat layer, wherein the surface resin layer is provided on one side of the base layer, and a concave-convex pattern is provided on the surface resin layer, and the gel coat layer is provided on the other side of the base layer, and the base layer comprises the following raw materials in parts by weight: 4 parts of continuous reinforcement layer, 102 parts of unsaturated polyester resin A, 2 parts of curing agent A, 0.22 parts of initiator A, 0.12 parts of inhibitor A, and 13.36 parts of skeleton material; the gel coat layer comprises the following raw materials in parts by weight: 106 parts of unsaturated polyester resin B, 9.8 parts of flexible unsaturated resin, 2 parts of curing agent B, 0.9 parts of initiator B, 1.34 parts of defoaming agent, 1.26 parts of leveling agent, 0.37 parts of inhibitor B, and 6.4 parts of chain agent;

[0060] Preferably, the continuous reinforcement layer is any one of surface felt, glass fiber chopped yarn, chopped strand mat, woven cloth, glass fiber felt, glass fiber cloth, carbon fiber, basalt fiber, multi-axial cloth, stitched felt, and warp knitted cloth, or a combination of at least two of them.

[0061] Specifically, the continuous reinforcement layer is 1 part of glass fiber chopped yarn, 0.6 part of glass fiber mat, and 0.4 part of stitched mat; the unsaturated polyester resin A is isophthalic unsaturated polyester resin; the curing agent A is methyl ethyl ketone peroxide; the initiator A is a cobalt-based initiator; the inhibitor A is DPPH, TBC, phenol, and ferric chloride, and the ratio of DPPH, TBC, phenol and ferric chloride is 1:1:1:1; the chain agent is 6.4 parts. The chain agent is hydrogenated bisphenol A. The depth of the concave-convex pattern is 300-500um.

[0062] Preferably, the skeleton material is any one or a combination of at least two of aluminum hydroxide, diatomaceous earth, talc, kaolin, hollow microspheres, cellulose, ceramic powder, mica, and pearl powder. Specifically, 3.6 parts of cellulose, 2.66 parts of pearl powder, and 7.4 parts of mica.

[0063] Specifically, the unsaturated polyester resin B is an isophthalic unsaturated polyester resin, the flexible unsaturated resin is an orthophthalic unsaturated polyester resin; the curing agent B is methyl ethyl ketone peroxide; the initiator B is a cobalt-based initiator; the defoamer is a polysiloxane carbon-based compound or a GPES polyether defoamer; the leveling agent is a modified polysiloxane compound; the inhibitor B is PPH, TBC, phenol, and ferric chloride, and the dosage ratio of DPPH, TBC, phenol, and ferric chloride is 1:1:1:1. The outer surface of the gel coat layer is provided with a concave-convex pattern with a depth of 50±10um.

[0064] The present invention provides a method for preparing the glass fiber reinforced plastic sheet as described above, comprising the following steps:

[0065] (2) unsaturated polyester resin A, curing agent A, initiator A, chain scission agent and polymerization inhibitor A are mixed to obtain a matrix raw material mixed liquid, and the matrix raw material mixed liquid is applied layer by layer to infiltrate the continuous reinforcement layer to obtain a glass fiber reinforced plastic sheet precursor;

[0066] Specifically, step (1) includes the following specific steps:

[0067] (1-1) Preparation of gel coat layer: unsaturated polyester resin B, flexible unsaturated resin, curing agent B, initiator B, defoamer, leveling agent, and inhibitor B are mixed to obtain gel coat layer raw material liquid, the gel coat layer raw material liquid is sprayed onto the base film of gel coat layer, and heated and cured to obtain gel coat layer;

[0068] (1-2) Unsaturated polyester resin A, curing agent A, initiator A, inhibitor A, chain-binding agent and skeleton material are mixed to obtain a matrix raw material mixed liquid, and the matrix raw material mixed liquid is coated layer by layer on the surface of the gel coat layer to infiltrate the continuous reinforcement layer to obtain a glass fiber reinforced plastic sheet precursor containing a gel coat layer. (2) Unsaturated polyester resin C is first coated on the bonding surface of the glass fiber reinforced plastic sheet precursor, and the unsaturated polyester resin C includes a chain-binding agent to form a surface resin layer, and then a base film is bonded, and then the surface is passed through a patterned roller track, and finally rolling, heating and curing and negative pressure heating are performed in sequence to obtain a glass fiber reinforced plastic sheet with a concave and convex pattern.

[0069] Specifically, in step (2), the unsaturated polyester resin C further comprises isophthalic unsaturated polyester resin and vinyl resin, and the weight ratio of the isophthalic unsaturated polyester resin to the vinyl resin is 0.3 Kg / m 2 ; The temperature of heating curing is 80-135℃; the temperature of negative pressure heating is 80 and the pressure is 30KPa.

[0070] In step (1-1), the temperature for heating and curing is 80-135°C.

[0071] Example 3

[0072] The present embodiment relates to a glass fiber reinforced plastic sheet, comprising a base layer and a surface resin layer, wherein the surface resin layer is provided on one side of the base layer, and the surface resin layer is provided with a concave-convex pattern, wherein the base layer comprises the following raw materials in parts by weight: 3 parts of a continuous reinforcement layer, 102 parts of an unsaturated polyester resin A, 2 parts of a curing agent A, 0.22 parts of an initiator A, 0.12 parts of an inhibitor A, and 13.36 parts of a skeleton material, and the surface resin layer comprises the following raw materials in parts by weight: 6.4 parts of a chain agent;

[0073] Preferably, the continuous reinforcement layer is any one of surface felt, glass fiber chopped yarn, chopped strand mat, woven cloth, glass fiber felt, glass fiber cloth, carbon fiber, basalt fiber, multi-axial cloth, stitched felt, and warp knitted cloth, or a combination of at least two of them.

[0074] Specifically, the continuous reinforcement layer is 1 part of glass fiber chopped yarn, 0.6 part of glass fiber mat, and 0.4 part of stitched mat; the unsaturated polyester resin A is isophthalic unsaturated polyester resin; the curing agent A is methyl ethyl ketone peroxide; the initiator A is a cobalt-based initiator; the inhibitor A is DPPH, TBC, phenol, and ferric chloride, and the ratio of DPPH, TBC, phenol and ferric chloride is 1:1:1:1; the chain agent is 6.4 parts. The chain agent is ethylene glycol.

[0075] Wherein, the depth of the concave-convex pattern is 300-500um.

[0076] Preferably, the skeleton material is any one or a combination of at least two of aluminum hydroxide, diatomaceous earth, talc, kaolin, hollow microspheres, cellulose, ceramic powder, mica, and pearl powder; specifically, 3.6 parts of cellulose, 2.66 parts of pearl powder, and 7.4 parts of mica.

[0077] The present invention provides a method for preparing the glass fiber reinforced plastic sheet as described above, comprising the following steps:

[0078] (1) unsaturated polyester resin A, curing agent A, initiator A, polymerization inhibitor A, chain scission agent and skeleton material are mixed to obtain a matrix raw material mixed liquid, and the matrix raw material mixed liquid is applied layer by layer to infiltrate the continuous reinforcement layer to obtain a glass fiber reinforced plastic sheet precursor;

[0079] (2) First, one side of the glass fiber reinforced plastic sheet precursor is coated with unsaturated polyester resin C, wherein the unsaturated polyester resin C includes a chain-binding agent to form a surface resin layer, and then a concave-convex pattern film is bonded thereto, and then rolling, heating and curing, and negative pressure heating are performed in sequence to obtain a glass fiber reinforced plastic sheet with a concave-convex pattern.

[0080] Specifically, in step (2), the unsaturated polyester resin C further comprises isophthalic unsaturated polyester resin and vinyl resin, and the weight ratio of the isophthalic unsaturated polyester resin to the vinyl resin is 0.3 Kg / m 2 ; The temperature for heating and curing is 80-135℃; the temperature for negative pressure heating is 80℃ and the pressure is 30KPa.

[0081] Example 4

[0082] The present embodiment relates to a glass fiber reinforced plastic sheet, comprising a base layer and a surface resin layer, wherein the surface resin layer is provided on one side of the base layer, and the surface resin layer is provided with a concave-convex pattern, wherein the base layer comprises the following raw materials in parts by weight: 3 parts of a continuous reinforcement layer, 102 parts of an unsaturated polyester resin A, 2 parts of a curing agent A, 0.22 parts of an initiator A, 0.12 parts of an inhibitor A, and 13.36 parts of a skeleton material, and the surface resin layer comprises the following raw materials in parts by weight: 6.4 parts of a chain agent;

[0083] Preferably, the continuous reinforcement layer is any one of surface felt, glass fiber chopped yarn, chopped strand mat, woven cloth, glass fiber felt, glass fiber cloth, carbon fiber, basalt fiber, multi-axial cloth, stitched felt, and warp knitted cloth, or a combination of at least two of them.

[0084] Specifically, the continuous reinforcement layer is 1 part of glass fiber chopped yarn, 0.6 part of glass fiber mat, and 0.4 part of stitched mat; the unsaturated polyester resin A is isophthalic unsaturated polyester resin; the curing agent A is methyl ethyl ketone peroxide; the initiator A is a cobalt-based initiator; the inhibitor A is DPPH, TBC, phenol, and ferric chloride; the chain scissor is 6.4 parts. The chain scissor is trimethylolpropane.

[0085] Wherein, the depth of the concave-convex pattern is 300-500um.

[0086] Preferably, the skeleton material is any one or a combination of at least two of aluminum hydroxide, diatomaceous earth, talc, kaolin, hollow microspheres, cellulose, ceramic powder, mica, and pearl powder; specifically, 3.6 parts of cellulose, 2.66 parts of pearl powder, and 7.4 parts of mica.

[0087] The present invention provides a method for preparing the glass fiber reinforced plastic sheet as described above, comprising the following steps:

[0088] (1) unsaturated polyester resin A, curing agent A, initiator A, polymerization inhibitor A, chain scission agent and skeleton material are mixed to obtain a matrix raw material mixed liquid, and the matrix raw material mixed liquid is applied layer by layer to infiltrate the continuous reinforcement layer to obtain a glass fiber reinforced plastic sheet precursor;

[0089] (2) The bonding surface of the FRP sheet precursor is first coated with unsaturated polyester resin C, wherein the unsaturated polyester resin C includes a chain-binding agent to form a surface resin layer, and then bonded to a base film, and then passed through a patterned roller belt, and finally subjected to rolling, heating curing and negative pressure heating in sequence to obtain a FRP sheet with a concave-convex pattern.

[0090] Specifically, in step (2), the unsaturated polyester resin C further comprises isophthalic unsaturated polyester resin and vinyl resin, and the weight ratio of the isophthalic unsaturated polyester resin to the vinyl resin is 0.3 Kg / m 2 ; The temperature for heating and curing is 80-135℃; the temperature for negative pressure heating is 80℃ and the pressure is 30KPa.

[0091] Comparative Example 1

[0092] Compared with Example 1, in the production process, a common film is used, but a patterned roller track is used, and the rest is the same as Example 1.

[0093] Comparative Example 2

[0094] Compared with Example 1, no chain-building agent is used in the production process, and the rest is the same as Example 1.

[0095] Comparative Example 3

[0096] Compared with Example 1, in the production process, no chain agent is used, but a patterned roller track is used, and the rest is the same as Example 1.

[0097] Test example

[0098] The method for preparing the composite board according to the present invention comprises the following steps:

[0099] 1. Make the black material (polyurethane rigid foam combined polyether) and the white material (polymerized MDI) into prepolymer;

[0100] 2. Apply the semi-finished prepolymer product evenly on the inner surface of the fiberglass reinforced plastic sheet, and press the inner surface of the cover plate inward;

[0101] 3. At room temperature 25 degrees Celsius, the pressure is 0.5-0.1kg / cm 2 , maintain pressure for 4 hours to allow it to mature and solidify.

[0102] 4. Packing to obtain composite board.

[0103] The obtained composite board was tested for blister rate and pull-out force, and the testing method was as follows: (1) blister rate: GB / T 10802-1989; (2) pull-out force: GB / T 2791-1995; (3) production efficiency: production time used for producing every 100 sets of boards. The test results are shown in Table 1.

[0104] Table 1 Experimental results of blister rate and pull-out force of Examples 1-4 and Comparative Example 1

[0105]

[0106] Table 1 shows that the composite board of the present invention is much stronger than ordinary boards in practical strength. The higher the blister rate and the pull-out force, the more stable the composite board is, the longer the service life is, the wider the application field is, and the greater the practical advantages are. Since the fiberglass reinforced plastic board adopts the skeleton material, it is lighter than the ordinary board.

[0107] In summary, the FRP sheet of the present invention is an integral flat plate, and a concave-convex pattern is formed on one side of the base layer, so that the entire FRP sheet has a friendly bonding interface; when it is applied to downstream products of FRP panels, such as polyurethane foaming integrated composite process, on the one hand, the polyurethane foam material and the base layer can be integrated, the contact area between the base layer and the polyurethane foam material can be increased, and the polyurethane foam material can enter the interior of the concave-convex pattern to produce a vertical structure, and the chain agent can react with the functional groups on the linear polymer chain to expand the molecular chain and increase the molecular weight, thereby improving the adhesion between the two and avoiding serious quality defects such as bulging and delamination to a large extent; another invention is that the concave-convex pattern of the base layer improves the fluidity of the foaming process and increases the blister rate of the bonding surface with the polyurethane foam material, thereby achieving deep composite of the FRP sheet and the polyurethane foam; thereby improving the poor bonding effect of the existing foaming composite process and serious quality defects such as bulging and delamination.

[0108] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0109] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A glass fiber reinforced plastic sheet, characterized in that: The invention comprises a base layer and a surface resin layer, wherein the surface resin layer is arranged on one side of the base layer, and the surface resin layer is provided with a concave-convex pattern, wherein the base layer comprises the following raw materials in parts by weight: 1-5 parts of a continuous reinforcement layer, 51-153 parts of an unsaturated polyester resin A, 1-3 parts of a curing agent A, 0.11-0.33 parts of an initiator A, and 0.06-0.18 parts of an inhibitor A; and the surface resin layer comprises the following raw materials in parts by weight: 1.35-9.6 parts of a chain scissor agent; The chain-building agent includes any one of ethylene glycol, propylene glycol, 1,4-butanediol, diethylene glycol, glycerol, trimethylolpropane, 1,4-cyclohexanediol, hydrogenated bisphenol A, dimethylbenzene glycol, hydroquinone bis-β-hydroxyethyl ether, resorcinol hydroxy ether, diethanolamine, triethanolamine, methyldiethanolamine, diethyltoluenediamine, 3,5-dimethylthiotoluenediamine, or a combination of at least two thereof; the depth of the concave-convex pattern is 300-500um; The preparation method of the glass fiber reinforced plastic plate comprises the following steps: (1) unsaturated polyester resin A, curing agent A, initiator A and inhibitor A are mixed to obtain a matrix raw material mixed liquid, and the matrix raw material mixed liquid is applied layer by layer to infiltrate the continuous reinforcement layer to obtain a glass fiber reinforced plastic sheet precursor; (2) firstly coating one side of the glass fiber reinforced plastic sheet precursor with an unsaturated polyester resin C, wherein the unsaturated polyester resin C includes a chain-binding agent, to form a surface resin layer, and then bonding a concave-convex pattern film, and then sequentially performing roller pressing, heating curing and negative pressure heating to obtain a glass fiber reinforced plastic sheet with a concave-convex pattern; Or, firstly, one side of the glass fiber reinforced plastic sheet precursor is coated with unsaturated polyester resin C, wherein the unsaturated polyester resin C includes a chain-binding agent, to form a surface resin layer, and then a base film is bonded thereto, and then the surface is passed through a patterned roller track, and finally roller pressing, heating curing and negative pressure heating are performed in sequence to obtain a glass fiber reinforced plastic sheet with a concave-convex pattern; The unsaturated polyester resin A includes isophthalic unsaturated polyester resin; the curing agent A includes methyl ethyl ketone peroxide; the initiator A includes a cobalt-based initiator; the inhibitor A includes any one of DPPH, TBC, phenol, and ferric chloride, or a combination of at least two thereof; The unsaturated polyester resin C also includes isophthalic unsaturated polyester resin or vinyl resin.

2. The glass fiber reinforced plastic sheet according to claim 1, characterized in that: The continuous reinforcement layer includes any one of surface mat, glass fiber chopped yarn, chopped mat, woven cloth, glass fiber mat, glass fiber cloth, carbon fiber, basalt fiber, multi-axial cloth, stitched mat, and warp knitted cloth, or a combination of at least two of them.

3. A glass fiber reinforced plastic sheet according to claim 1 or 2, characterized in that: The base layer also includes 6.68-20.04 parts of a skeleton material; the skeleton material includes any one of aluminum hydroxide, diatomaceous earth, talc, kaolin, hollow microspheres, cellulose, ceramic powder, mica, and pearl powder, or a combination of at least two of them.

4. A glass fiber reinforced plastic sheet according to claim 1 or 2, characterized in that: The glass fiber reinforced plastic sheet also includes a gel coat layer, which is arranged on the other side of the base layer. The gel coat layer includes the following raw materials in parts by weight: unsaturated polyester resin B 53-159 parts, 4.9-14.7 parts of flexible unsaturated resin, 1-3 parts of curing agent B, 0.45-1.35 parts of initiator B, 0.67-2.01 parts of defoaming agent, 0.63-1.89 parts of leveling agent, and 0.185-0.555 parts of inhibitor B; the unsaturated polyester resin B includes isophthalic unsaturated polyester resin, and the flexible unsaturated resin includes orthophthalic unsaturated polyester resin; the curing agent B includes methyl ethyl ketone peroxide; the initiator B includes a cobalt-based initiator; the defoaming agent includes a polysiloxane carbon-based compound or a GPES polyether defoaming agent; the leveling agent includes a modified polysiloxane compound; the inhibitor B includes any one of DPPH, TBC, phenol, and ferric chloride or a combination of at least two thereof; the outer surface of the gel coat layer is provided with a concave-convex texture with a depth of 50±10 um; step (1) includes the following specific steps: (1-1) Preparation of gel coat layer: unsaturated polyester resin B, flexible unsaturated resin, curing agent B, initiator B, defoamer, leveling agent, and inhibitor B are mixed to obtain gel coat layer raw material liquid, the gel coat layer raw material liquid is sprayed onto the base film of gel coat layer, and heated and cured to obtain gel coat layer; (1-2) Unsaturated polyester resin A, curing agent A, initiator A, inhibitor A and skeleton material are mixed to obtain a matrix raw material mixed liquid, and the matrix raw material mixed liquid is applied layer by layer on the surface of the gel coat layer to infiltrate the continuous reinforcement layer to obtain a glass fiber reinforced plastic sheet precursor containing a gel coat layer.

5. The glass fiber reinforced plastic sheet according to claim 4, characterized in that: The temperature for heating curing is 80-135℃; the temperature for negative pressure heating is 85℃ and the pressure is 15-40KPa; In step (1-1), the temperature for heating and curing is 80-135°C.

6. A composite board, characterized in that: It comprises the glass fiber reinforced plastic sheet as claimed in any one of claims 1 to 4.

7. The composite plate according to claim 6, characterized in that: The composite board comprises an upper surface layer, a lower surface layer and a core layer which are integrally formed, the core layer is arranged between the upper surface layer and the lower surface layer, the upper surface layer and the lower surface layer are both the glass fiber reinforced plastic sheet materials, and the core layer is polyurethane foam.

8. An application of the composite board according to any one of claims 6 to 7, characterized in that: The composite plate is used in cold chain logistics.