Titanium-free silver-white pearlescent pigment and preparation method and use thereof

By covering the titanium-free silver-white pearlescent pigment with magnesium oxide layer and metal oxide layer on the surface of the substrate, the color change and regulatory restrictions in cosmetics are solved, and excellent UV resistance and pearlescent effect are achieved, suitable for cosmetics and individuals Care products.

CN117624942BActive Publication Date: 2024-11-26GUANGXI CHESIR PEARL MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311661907.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-05
Publication Date
2024-11-26
Estimated Expiration
2043-12-05

AI Technical Summary

Technical Problem

Existing pearlescent pigments have color change and color migration in the cosmetics field, and pearlescent pigments containing titanium do not meet relevant regulations, especially under strict EU regulations.

Method used

Using the titanium-free silver-white pearlescent pigment design, the magnesium oxide layer, metal oxide layer and protective layer are coated on the surface of the substrate to prepare a pearlescent pigment without titanium, which has excellent UV resistance and good gloss.

Benefits of technology

Overcome color change and color migration problems, meet regulatory requirements, provide good pearlescent effect and light resistance, is suitable for cosmetics and personal care products, and the titanium-free design avoids potential safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117624942B_ABST
    Figure CN117624942B_ABST
Patent Text Reader

Abstract

The invention discloses a titanium-free silver-white pearlescent pigment, a preparation method and application thereof. The pearlescent pigment of the invention has obvious pearlescent effect, rich particle sizes, and gloss ranging from soft to very shiny. It can be widely used in multiple fields, especially in the fields of cosmetics and personal care products, and has good practical value. In addition, the pearlescent pigment does not contain titanium, has excellent ultraviolet resistance, and overcomes the color change and color migration problems of conventional titanium-containing pearlescent pigments in the production and application of cosmetics. In addition, the pearlescent pigment also has the advantages of simple preparation process, easy availability of raw materials, convenient processing operation, etc., and can be applied to large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a pearlescent pigment, in particular to a titanium-free silver-white pearlescent pigment and a preparation method and application thereof, belonging to the technical field of pearlescent pigment production. Background Art

[0002] Pearlescent pigments, with their unique optical properties and color effects, have been widely used in coatings, plastics, ceramics, leather, cosmetics, decorative materials and other fields. Especially in recent years, they have been shining in the field of cosmetics and personal care products, such as lip gloss, eye shadow, powder, nail polish, lotion, face cream, shampoo, conditioner, etc. The main function is to keep the skin in good condition by beautifying, cleaning or protecting, to avoid dry skin or damage by ultraviolet rays, so as to maintain skin health.

[0003] At present, the pearlescent pigment products launched by domestic and foreign pearlescent pigment manufacturers on the market are usually formed by coating two or more metal oxides on the surface of the substrate in terms of film structure, thus forming a layered sandwich structure. Such as: substrate flakes / TiO2, substrate flakes / SnO2 / TiO2, substrate flakes / Fe2O3, substrate flakes / SnO2 / TiO2 / Fe2O3, pearlescent pigment / organic pigment and other structures derived therefrom; these are basically mica titanium, mica iron or mica titanium / iron pearlescent pigments and their derivatives, which are generally formed by coating TiO2, Fe2O3, TiO2 / Fe2O3, etc. The nano-TiO2 on the pearlescent pigment has the characteristics of strong photocatalytic performance, strong polarity, strong hydrophilicity, and poor visible light transmittance. Although it has good ultraviolet shielding ability, it has color change and color migration when used in the field of cosmetics and personal care products, which limits the application of pearlescent pigments in the field of cosmetics and personal care products.

[0004] Moreover, the EU has issued Commission Delegated Regulation (EU) 2020 / 217 of 4 October 2019 on February 18, 2020, which lists TiO2 as a Class II carcinogen and requires that "solid mixtures containing 1% or more of TiO2 must be labeled accordingly on the packaging". This regulation will be implemented on September 9, 2021. On January 14, 2022, the EU issued Commission Regulation (EU) 2022 / 63 prohibiting the use of TiO2 (E171) as a food additive, which restricts the application of TiO2 in the fields of medicine and food. In June 2022, the European Health and Food Safety Committee solicited opinions on the safety of using TiO2 in cosmetics. The main content includes that the Scientific Committee on Consumer Safety (SCCS) re-evaluated TiO2 in view of its classification as a Class 2 carcinogen only through inhalation. The focus is on genotoxicity and exposure via inhalation and oral routes (lip care, lipstick, toothpaste, loose powder, hair spray), as well as seeking opinions on whether TiO2 is safe for use in oral cosmetics, which will further restrict its use in cosmetics.

[0005] In summary, how to realize TiO2-free pearlescent pigments as cosmetic raw materials and meet the requirements of relevant regulations has become a technical problem that needs to be solved urgently. Summary of the invention

[0006] In view of the fact that titanium-containing pearlescent pigments in the prior art suffer from color change and color migration when used in the field of cosmetics and personal care products and fail to meet the strict requirements of relevant regulations, the present invention provides a titanium-free silver-white pearlescent pigment and a preparation method and use thereof. The pearlescent pigment of the present invention does not contain titanium and has excellent ultraviolet resistance, thereby overcoming the color change and color migration problems of conventional titanium-containing pearlescent pigments in the production and application of cosmetics.

[0007] In order to achieve the above technical objectives, the first embodiment of the present invention provides a titanium-free silver white pearlescent pigment:

[0008] A titanium-free silver-white pearlescent pigment comprises: a substrate, a magnesium oxide layer coated and deposited on the surface of the substrate, a high refractive index layer coated and deposited on the surface of the magnesium oxide layer, and a protective layer coated and deposited on the surface of the high refractive index layer.

[0009] Preferably, the substrate is one of mica, glass flakes, SiO2 flakes, Al2O3 flakes and bismuth oxychloride flakes, preferably one of mica flakes, glass flakes, SiO2 flakes, Al2O3 flakes and bismuth oxychloride flakes, more preferably natural mica powder or synthetic mica powder or glass flake powder.

[0010] Preferably, the high refractive index layer is a metal oxide layer with a refractive index greater than 1.8, and the metal oxide is preferably one of ZrO2, CeO2, and ZnO, and the metal oxide is more preferably CeO2 and / or ZnO.

[0011] Preferably, the protective layer is one or more of SiO2, Al2O3, and silane compounds, preferably SiO2 and / or Al2O3, and more preferably SiO2. Preferably, the silane compound is selected from one or more of (3-glycidyloxypropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane, methacrylpropylmethoxysilane, 3-(2-aminoethylamino)propyltrimethoxysilane, methyltriethoxysilane, and n-hexyltrimethoxysilane.

[0012] Preferably, the coverage of the magnesium oxide layer is 0.2-6%, preferably 0.5-5%, more preferably 1-4%, and further preferably 1.2-2.5%, for example, one of 0.2%, 0.3%, 0.5%, 0.8%, 1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 2%, 2.2%, 2.4%, 2.5%, 2.7%, 3%, 3.2%, 3.4%, 3.6%, 3.8%, 4%, 4.2%, 4.5%, 5%, 5.5%, and 6%.

[0013] Preferably, the coverage of the high refractive index layer is 10-45%, preferably 15-40%, more preferably 20-35%, for example, one of 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 34%, 36%, 38%, 40%, 42%, and 45%.

[0014] Preferably, the coverage of the protective layer is 0.05-7%, preferably 0.1-6%, more preferably 0.3-5%, for example, one of 0.05%, 0.08%, 0.1%, 0.12%, 0.15%, 0.18%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, and 7%.

[0015] Preferably, the thickness of the substrate is 50-500 nm, preferably 75-450 nm, and more preferably 100-400 nm.

[0016] Preferably, the particle size of the substrate is ≤500 μm, preferably ≤300 μm, and more preferably ≤250 μm.

[0017] According to a second embodiment of the present invention, a method for preparing a titanium-free silver-white pearlescent pigment is provided:

[0018] A method for preparing a titanium-free silver-white pearlescent pigment or a method for preparing a titanium-free silver-white pearlescent pigment as described in the first embodiment, the preparation method comprising:

[0019] 1) Dispersing the substrate in the dispersion to obtain a first suspension.

[0020] 2) adding a soluble magnesium salt solution to the first suspension to obtain a second suspension.

[0021] 3) Adding a soluble metal salt solution to the second suspension to obtain a third suspension.

[0022] 4) Adding a soluble protective salt solution to the third suspension to obtain a fourth suspension.

[0023] 5) The fourth suspension is filtered, washed, dried, calcined and sieved in sequence to obtain a titanium-free silver-white pearlescent pigment.

[0024] Preferably, the dispersion is deionized water, and the liquid-to-solid mass ratio of the dispersion to the added amount of the substrate is 3-20:1, preferably 5-15:1, and more preferably 7-12:1.

[0025] Preferably, the soluble magnesium salt is one or more of magnesium nitrate, magnesium sulfate, and magnesium chloride. The concentration of the soluble magnesium salt solution is 25-600 g / L, preferably 50-300 g / L, and more preferably 80-200 g / L. The amount of the soluble magnesium salt solution added is such that the coverage of the soluble magnesium salt on the surface of the substrate in the second suspension is 0.5-15%, preferably 0.8-12%, and more preferably 1-10%.

[0026] Preferably, the soluble metal salt is one or more of cerium nitrate, cerium chloride, cerium sulfate, zinc nitrate, zinc sulfate, and zinc chloride, preferably a mixed salt of one or more of cerium nitrate, cerium chloride, cerium sulfate and one or more of zinc nitrate, zinc sulfate, and zinc chloride, more preferably a mixed salt of cerium nitrate and zinc chloride.

[0027] Preferably, the concentration of the soluble metal salt solution is 80-700 g / L, preferably 100-500 g / L, and more preferably 120-300 g / L.

[0028] Preferably, the soluble metal salt solution is added in an amount such that the coverage rate of the soluble metal salt in the third suspension is 25-88%, preferably 30-80%, more preferably 35-75%.

[0029] Preferably, the soluble protective salt is one or more of aluminum chloride, aluminum nitrate, aluminum sulfate, sodium metasilicate pentahydrate, sodium metasilicate nonahydrate, and silane compounds, preferably aluminum chloride and / or sodium metasilicate pentahydrate, and more preferably sodium metasilicate pentahydrate.

[0030] Preferably, the concentration of the soluble protective salt solution is 30-250 g / L, preferably 40-200 g / L, and more preferably 50-180 g / L.

[0031] Preferably, the soluble protective salt solution is added in an amount such that the coverage rate of the soluble protective salt in the fourth suspension is 0.1-20%, preferably 0.5-15%, and more preferably 0.8-10%.

[0032] Preferably, step 1) is specifically as follows: disperse the substrate in the dispersion in proportion, stir and mix thoroughly, heat to 50-90° C. (preferably 75-85° C.) and keep the temperature constant, and use an acid or alkali (for example, a hydrochloric acid solution with a mass concentration of 5-18% or a sodium hydroxide solution with a mass concentration of 5-15%) to adjust the pH of the system to 7-9 (preferably 7.5-8.5) to obtain a first suspension.

[0033] Preferably, step 2) is specifically as follows: adding a soluble magnesium salt solution to the first suspension in proportion, controlling the temperature to 65-90°C (preferably 75-85°C), and using an acid or alkali (such as a hydrochloric acid solution with a mass concentration of 5-18% or a sodium hydroxide solution with a mass concentration of 5-15%) to adjust the system pH to 7-9 (preferably 7.5-8.5) to obtain a second suspension. And / or

[0034] Preferably, step 3) is specifically as follows: adding a soluble metal salt solution to the second suspension in proportion, controlling the temperature to 65-90°C (preferably 75-85°C), and using an acid or base (such as a hydrochloric acid solution with a mass concentration of 5-18% or a sodium hydroxide solution with a mass concentration of 5-15%) to adjust the system pH to 5-9 (preferably 5.5-8.5) to obtain a third suspension. And / or

[0035] Preferably, step 4) is specifically as follows: a soluble protective salt solution is added to the third suspension in proportion, the temperature is controlled to 65-90° C. (preferably 75-85° C.), and the pH of the system is adjusted to 7-10 (preferably 7.5-9) using an acid or alkali (for example, a hydrochloric acid solution with a mass concentration of 5-18% or a sodium hydroxide solution with a mass concentration of 5-15%) to obtain a fourth suspension.

[0036] Preferably, step 5) is as follows: the fourth suspension is filtered and washed, and then dried in an oven at 80-150°C (preferably 100-135°C). After drying, it is calcined at 700-900°C (preferably 750-850°C) for 1-15min (preferably 2-10min) and sieved to obtain a titanium-free silver white pearlescent pigment.

[0037] According to a third embodiment of the present invention, there is provided a use of a titanium-free silver white pearlescent pigment:

[0038] A use of a titanium-free silver-white pearlescent pigment or a use of a titanium-free silver-white pearlescent pigment as described in the first embodiment or a use of a titanium-free silver-white pearlescent pigment prepared by the method described in the second embodiment, wherein the titanium-free silver-white pearlescent pigment is used to prepare one or more of coatings, inks, plastics, and cosmetics. Preferably, the titanium-free silver-white pearlescent pigment is used to prepare one or more of lip gloss, eye shadow, powder, nail polish, lotion, face cream, shampoo, cleansing cream, and handmade soap.

[0039] In the present invention, the titanium-free silver-white pearlescent pigment of the present invention does not contain titanium. By sequentially coating and depositing a MgO layer, a metal oxide layer (such as a CeO2 layer, a ZnO layer, a ZnO / CeO2 layer\CeO2-ZnO composite layer), and an outermost protective layer (such as a SiO2 layer, an Al2O3 layer) on the surface of a substrate, a silver-white pearlescent pigment with excellent performance and good glossiness is prepared. The preparation method is simple, and titanium tetrachloride is not added during the preparation process, and there is no TiO2 component. The adverse effects of free radicals generated by TiO2 photocatalysis on the mica titanium pearlescent pigment and the coating / resin system in the application field, such as weakening of the pearlescent effect, discoloration, powdering, peeling, etc., can be overcome.

[0040] In the present invention, an MgO layer is added between the metal oxide layer and the substrate, and the MgO layer is used to inhibit the precipitation of oxygen vacancies in the metal oxide layer (such as CeO2 layer), thereby inhibiting the oxidation catalytic activity of the metal oxide, thereby improving the application of the titanium-free silver-white pearlescent pigment in various anti-ultraviolet fields such as anti-aging and cosmetics. The metal oxide is a cerium salt or a zinc salt, which is hydrolyzed and calcined to generate CeO2 and / or ZnO, and is an important deposition agent for the manufacture of mica pearlescent pigments; compared with the TiO2 component in the mica titanium pearlescent pigment, the CeO2 component in the titanium-free silver-white pearlescent pigment of the present invention has the following advantages: First, the refractive index of CeO2 is n=2.2, which is lower than that of TiO2 (gold red TiO2 n=2.72; anatase TiO2 n=2.5), better transmittance to visible light, plus its own soft color, not as white as TiO2, when used in cosmetics, it can make the skin whiteness appear more natural, without producing a "pale feeling", and the powder is smooth and has a better skin feel; secondly, CeO2 has a special 4f electron layer structure of rare earth, rich electron transition energy levels, sensitive to light absorption, and the absorption band is mostly in the ultraviolet region below 400nm, and the absorbed ultraviolet light is mainly used for electron energy level transition, reducing photocatalysis, and the photocatalytic performance is much lower than TiO2; plus the small size effect, high specific surface effect, and macroscopic quantum effect of nanoparticles, it has a strong scattering and reflection effect on ultraviolet light. Therefore, CeO2 has the dual functions of absorbing and reflecting ultraviolet rays, and the ultraviolet shielding efficiency is relatively high.

[0041] In the present invention, the outermost SiO2 and / or Al2O3 protective layer is a silicate or aluminum salt which is hydrolyzed and calcined to generate SiO 2、 Al2O3, this layer can cover the original optically active points of the pearlescent pigment and partially isolate the metal oxide layer from the effects of light, free H2O, and O2. Secondly, when the metal oxide layer is irradiated by light passing through the protective layer, the excited electrons pass through the defective lattices of SiO2 and Al2O3, and the SiO2 and Al2O3 layers absorb the excited electrons and recombine with holes, thereby reducing or blocking the number of electrons and holes reaching the surface of the metal oxide layer and improving the light resistance of the pearlescent pigment.

[0042] In the present invention, the coating thickness of the MgO layer is generally not more than 30nm (6-15nm). If the coating thickness of the MgO layer is too thin or the coating rate is too low (for example, less than 0.2%), it cannot well inhibit the oxidation catalytic activity of the metal oxide, affecting its anti-aging and anti-ultraviolet properties. If the coating thickness of the MgO layer is too thick or the coating rate is too high (for example, higher than 6%), it will occupy the thickness of the cerium oxide layer, which will weaken the pearlescent effect of the pearlescent pigment on the one hand, and also affect the ultraviolet shielding ability of the pearlescent pigment (the coating thickness is strongly correlated with the pearlescent effect of the pearlescent pigment. The thicker the thickness, the greater the deviation of hue, brightness and covering).

[0043] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0044] 1: The titanium-free silver-white pearlescent pigment of the present invention has excellent UV resistance, overcomes the color change and color migration problems of conventional mica titanium in the production and application of cosmetics, and the structural components do not contain TiO2, which can avoid a series of problems caused by future relevant regulations on "whether TiO2 or materials containing TiO2 components are safe for use in cosmetics or personal care products".

[0045] 2: The titanium-free silver-white pearlescent pigment provided by the present invention has obvious pearlescent effect, rich particle size, and brightness ranging from soft to shiny. It can be widely used in many fields, especially in the fields of cosmetics and personal care products, and has good practical value.

[0046] 3: The titanium-free silver-white pearlescent pigment provided by the present invention has the advantages of simple preparation process, readily available raw materials, convenient processing and operation, and can be applied to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is an electron microscope image (100 μm) of the pearlescent pigment obtained in Example 1 of the present invention.

[0048] Figure 2 This is an electron microscope image (20 μm) of the pearlescent pigment obtained in Example 1 of the present invention.

[0049] Figure 3 This is a screenshot of the SGS heavy metal test data report of the pearlescent pigment obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0050] The technical solution of the present invention is illustrated below by way of example, and the scope of protection requested by the present invention includes but is not limited to the following embodiments.

[0051] Example 1

[0052] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0053] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0054] The temperature of the second suspension was maintained and stably controlled at 80°C, and then a cerium nitrate solution with a concentration of 95 g / L was added, and at the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 53%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0055] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0056] The fourth suspension is vacuum filtered, the filter cake is washed with deionized water, and the filter cake is dried in an oven at 120°C; the dried filter cake powder is then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation is completed, the powder sample is taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the surface of the substrate are detected to be approximately 1.24%, 27.51%, and 0.97%, respectively).

[0057] Example 2

[0058] 100 g of natural mica powder with a particle size range of 10-70 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0059] A magnesium chloride solution with a concentration of 140 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0060] The temperature of the second suspension was maintained and stably controlled at 80° C., and then a 100 g / L cerium nitrate solution was added. At the same time, a 5% mass concentration of sodium hydroxide solution was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 55%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0061] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0062] The fourth suspension is vacuum filtered, the filter cake is washed with deionized water, and the filter cake is dried in an oven at 120°C; the dried filter cake powder is then placed in a muffle furnace, gradually heated to 850°C for calcination, and kept warm for 10 minutes. After the insulation is completed, the powder sample is taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the substrate surface are detected to be approximately 3.43%, 28.44%, and 0.94%, respectively).

[0063] Example 3

[0064] 100 g of glass flakes with a particle size range of 25-100 μm are taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0065] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0066] The temperature of the second suspension was maintained and stably controlled at 80°C, and then a cerium nitrate solution with a concentration of 95 g / L was added, and at the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 30%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0067] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 4.0%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0068] The fourth suspension is vacuum filtered, the filter cake is washed with deionized water, and the filter cake is dried in an oven at 120°C; the dried filter cake powder is then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation is completed, the powder sample is taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the surface of the substrate are detected to be approximately 1.21%, 13.37%, and 1.11%, respectively).

[0069] Example 4

[0070] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0071] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0072] The temperature of the second suspension was maintained and stably controlled at 80° C., and then a cerium nitrate solution with a concentration of 95 g / L was added, and a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of the cerium nitrate reached 40%, the addition was stopped, and stirring was continued for 20 minutes. Then, a zinc chloride solution with a concentration of 75 g / L was added, and the equilibrium pH value was adjusted to 6.5 with 10% dilute hydrochloric acid. When the coverage rate of the zinc chloride reached 11%, the addition was stopped, and stirring was continued for 20 minutes to obtain a third suspension.

[0073] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0074] The fourth suspension is vacuum filtered, the filter cake is washed with deionized water, and the filter cake is dried in an oven at 120°C; the dried filter cake powder is then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation is completed, the powder sample is taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the surface of the substrate are detected to be approximately 1.22%, 27.60%, and 0.98%, respectively).

[0075] Example 5

[0076] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0077] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0078] The temperature of the second suspension was maintained and stably controlled at 80° C., and then a mixed solution of cerium nitrate with a concentration of 95 g / L and zinc chloride with a concentration of 75 g / L was added. At the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the total coating rate of cerium nitrate-zinc chloride reached 51%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0079] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0080] The fourth suspension is vacuum filtered, the filter cake is washed with deionized water, and the filter cake is dried in an oven at 120°C; the dried filter cake powder is then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation is completed, the powder sample is taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the surface of the substrate are detected to be approximately 1.26%, 27.55%, and 0.96%, respectively).

[0081] Example 6

[0082] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0083] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 5%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0084] The temperature of the second suspension was maintained and stably controlled at 80°C, and then a cerium nitrate solution with a concentration of 95 g / L was added, and at the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 53%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0085] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0086] The fourth suspension is vacuum filtered, the filter cake is washed with deionized water, and the filter cake is dried in an oven at 120°C; the dried filter cake powder is then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation is completed, the powder sample is taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the surface of the substrate are detected to be approximately 2.05%, 27.49%, and 0.98%, respectively).

[0087] Example 7

[0088] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0089] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 6%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0090] The temperature of the second suspension was maintained and stably controlled at 80°C, and then a cerium nitrate solution with a concentration of 95 g / L was added, and at the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 53%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0091] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0092] The fourth suspension is vacuum filtered, the filter cake is washed with deionized water, and the filter cake is dried in an oven at 120°C; the dried filter cake powder is then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation is completed, the powder sample is taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the surface of the substrate are detected to be approximately 2.46%, 27.50%, and 0.99%, respectively).

[0093] Example 8

[0094] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0095] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 1%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0096] The temperature of the second suspension was maintained and stably controlled at 80°C, and then a cerium nitrate solution with a concentration of 95 g / L was added, and at the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 53%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0097] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0098] The fourth suspension is vacuum filtered, the filter cake is washed with deionized water, and the filter cake is dried in an oven at 120°C; the dried filter cake powder is then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation is completed, the powder sample is taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the surface of the substrate are detected to be approximately 0.41%, 27.52%, and 0.97%, respectively).

[0099] Example 9

[0100] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0101] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0102] The temperature of the second suspension was maintained and stably controlled at 80° C., and then a zinc chloride solution with a concentration of 75 g / L was added. At the same time, a dilute hydrochloric acid solution with a mass concentration of 5% was used to balance the pH value to 6.5. When the coverage rate of zinc chloride reached 47%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0103] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0104] The fourth suspension is vacuum filtered, the filter cake is washed with deionized water, and the filter cake is dried in an oven at 120°C; the dried filter cake powder is then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation is completed, the powder sample is taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the surface of the substrate are detected to be approximately 1.22%, 27.57%, and 0.99%, respectively).

[0105] Example 10

[0106] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0107] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0108] The temperature of the second suspension was maintained and stably controlled at 80°C, and then a zirconium nitrate solution with a concentration of 95 g / L was added. At the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of the zirconium nitrate reached 77%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0109] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0110] The fourth suspension was vacuum filtered, the filter cake was washed with deionized water, and the filter cake was dried in an oven at 120°C; the dried filter cake powder was then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation was completed, the powder sample was taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the surface of the substrate were detected to be approximately 1.25%, 27.59%, and 0.97%, respectively).

[0111] Embodiment 11

[0112] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0113] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0114] The temperature of the second suspension was maintained and stably controlled at 80° C., then a zinc chloride solution with a concentration of 75 g / L was added, and a 10% dilute hydrochloric acid was used to adjust the equilibrium pH value to 6.5. When the coverage rate of zinc chloride reached 11%, the addition was stopped, and stirring was continued for 20 minutes. Then, a cerium nitrate solution with a concentration of 95 g / L was added, and a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 40%, the addition was stopped, and stirring was continued for 20 minutes to obtain a third suspension.

[0115] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0116] The fourth suspension is vacuum filtered, the filter cake is washed with deionized water, and the filter cake is dried in an oven at 120°C; the dried filter cake powder is then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation is completed, the powder sample is taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment with a silvery white appearance (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the surface of the substrate are detected to be approximately 1.22%, 27.55%, and 0.98%, respectively).

[0117] Example 12

[0118] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0119] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 18%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0120] The temperature of the second suspension was maintained and stably controlled at 80°C, and then a cerium nitrate solution with a concentration of 95 g / L was added, and at the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 53%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0121] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0122] The fourth suspension was vacuum filtered, the filter cake was washed with deionized water, and the filter cake was dried in an oven at 120°C; the dried filter cake powder was then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation was completed, the powder sample was taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the substrate surface were detected to be approximately 7.51%, 27.54%, and 0.98%, respectively).

[0123] Embodiment 13

[0124] Example 12 was repeated except that the coverage of magnesium chloride was 0.4% (the coverage of the magnesium oxide layer, high refractive index layer and protective layer on the substrate surface was detected to be approximately 0.16%, 27.58% and 0.97%, respectively).

[0125] Embodiment 14

[0126] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0127] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0128] The temperature of the second suspension was maintained and stably controlled at 80°C, and then a cerium nitrate solution with a concentration of 95 g / L was added, and at the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of the cerium nitrate reached 10%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0129] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0130] The fourth suspension was vacuum filtered, the filter cake was washed with deionized water, and the filter cake was dried in an oven at 120°C; the dried filter cake powder was then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation was completed, the powder sample was taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment (the coverage rates of the magnesium oxide layer, the high refractive index layer, and the protective layer on the substrate surface were detected to be approximately 1.23%, 5.19%, and 0.99%, respectively).

[0131] Embodiment 15

[0132] Example 1 was repeated except that the sodium metasilicate pentahydrate was replaced by aluminum chloride.

[0133] Example 16

[0134] Example 1 was repeated except that cerium nitrate was replaced by cerium chloride.

[0135] Embodiment 17

[0136] Example 1 was repeated except that zinc chloride was replaced by zinc nitrate.

[0137] Embodiment 18

[0138] Example 1 was repeated except that the magnesium chloride was replaced by magnesium sulfate.

[0139] Comparative Example 1

[0140] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0141] The temperature of the first suspension was maintained and stably controlled at 80° C. A 95 g / L cerium nitrate solution was added to the first suspension using a peristaltic pump. A 5% mass concentration of sodium hydroxide solution was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 53%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0142] The temperature of the second suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0143] The third suspension was vacuum filtered, the filter cake was washed with deionized water, and the filter cake was dried in an oven at 120°C; the dried filter cake powder was then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation was completed, the powder sample was taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment (the coverage of the high refractive index layer and the protective layer on the substrate surface were detected to be approximately 27.50% and 0.96%, respectively).

[0144] Comparative Example 2

[0145] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0146] A 135 g / L calcium chloride solution was added to the first suspension by a peristaltic pump, and a 5% mass concentration sodium hydroxide solution was used to keep the pH constant. When the calcium chloride coating rate reached 2.6%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0147] The temperature of the second suspension was maintained and stably controlled at 80°C, and then a cerium nitrate solution with a concentration of 95 g / L was added, and at the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 53%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0148] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0149] The fourth suspension was vacuum filtered, the filter cake was washed with deionized water, and the filter cake was dried in an oven at 120°C; the dried filter cake powder was then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation was completed, the powder sample was taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment (the coverage rates of the calcium oxide layer, high refractive index layer, and protective layer on the substrate surface were detected to be approximately 1.26%, 27.55%, and 0.99%, respectively).

[0150] Comparative Example 3

[0151] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0152] A 95 g / L cerium nitrate solution was added to the first suspension using a peristaltic pump, and a 5% sodium hydroxide solution was used to balance the pH to 8.0. When the coverage of cerium nitrate reached 53%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0153] The temperature of the second suspension was maintained and stably controlled at 80° C., and then a magnesium chloride solution with a concentration of 135 g / L was added. At the same time, a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0154] The temperature of the third suspension was maintained and stably controlled at 80° C., and then a 100 g / L sodium metasilicate pentahydrate solution was added. At the same time, a 5% mass concentration of hydrochloric acid solution was used to balance the pH value to 8.0. When the coverage rate of sodium metasilicate pentahydrate reached 3.5%, the addition was stopped and stirring was continued for 20 minutes to obtain a fourth suspension.

[0155] The fourth suspension was vacuum filtered, the filter cake was washed with deionized water, and the filter cake was dried in an oven at 120°C; the dried filter cake powder was then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation was completed, the powder sample was taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment (the coverage rates of the high refractive index layer, magnesium oxide layer, and protective layer on the substrate surface were detected to be approximately 27.53%, 1.22%, and 0.99%, respectively).

[0156] Comparative Example 4

[0157] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 80° C., and the pH of the suspension is adjusted to 7.5 with 15% dilute hydrochloric acid to obtain a first suspension;

[0158] A magnesium chloride solution with a concentration of 135 g / L was added to the first suspension by a peristaltic pump, and a sodium hydroxide solution with a mass concentration of 5% was used to keep the pH constant. When the magnesium chloride coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0159] The temperature of the second suspension was maintained and stably controlled at 80°C, and then a cerium nitrate solution with a concentration of 95 g / L was added, and at the same time, a sodium hydroxide solution with a mass concentration of 5% was used to balance the pH value to 8.0. When the coverage rate of cerium nitrate reached 53%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0160] The third suspension was vacuum filtered, the filter cake was washed with deionized water, and the filter cake was dried in an oven at 120°C; the dried filter cake powder was then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation was completed, the powder sample was taken out and naturally cooled to room temperature, then washed and dried to obtain a pearlescent pigment (the coverage rates of the magnesium oxide layer and the high refractive index layer on the substrate surface were detected to be approximately 1.24% and 27.57%, respectively).

[0161] Comparative Example 5

[0162] 100 g of synthetic mica powder with a particle size range of 10-60 μm is taken and put into a reactor with a capacity of 2 L, deionized water is added at a solid-liquid mass ratio of 1:10, and the mixture is stirred evenly to form a suspension; the suspension is heated in a constant temperature water bath and stabilized at 65° C., and the pH of the suspension is adjusted to 1.5 with dilute hydrochloric acid with a mass concentration of 15%, thereby obtaining a first suspension;

[0163] A 235 g / L tin chloride solution was added to the first suspension by a peristaltic pump, and the pH value was not constant. When the SnO2 coating rate reached 3%, the addition was stopped and stirring was continued for 20 minutes to obtain a second suspension.

[0164] The temperature of the second suspension was adjusted and stably controlled at 80°C, the pH value was adjusted to 1.8 with 30% sodium hydroxide by mass concentration, and 2 mol / L titanium tetrachloride solution was added. At the same time, the pH value was balanced to 1.8 with 30% sodium hydroxide by mass concentration. When the coverage rate of TiO2 reached 25%, the addition was stopped and stirring was continued for 20 minutes to obtain a third suspension.

[0165] The third suspension was vacuum filtered, the filter cake was washed with deionized water, and the filter cake was dried in an oven at 120°C. The dried filter cake powder was then placed in a muffle furnace, gradually heated to 800°C for calcination, and kept warm for 10 minutes. After the insulation was completed, the powder sample was taken out and naturally cooled to room temperature, and then washed and dried to obtain a mica titanium pearlescent pigment with a silvery white appearance.

[0166] Effect test example 1

[0167] The pearlescent pigment powders obtained in the above Examples 1-14 and Comparative Examples 1-5 were coated on a card and the dispersibility was observed. Then the data were tested using X-Rite MA98. The results are shown in Table 1 below:

[0168] Table 1:

[0169]

[0170]

[0171] It can be seen that the color data of Examples 1-14 and Comparative Examples 1-5 are basically the same, and the hues are basically consistent. The difference lies in the deposition agents and their coverage rates.

[0172] The D65 / 10°Lab data measured by the X-Rite MA98 colorimeter is shown in Table 2 below:

[0173] Table 2:

[0174]

[0175]

[0176] Wherein, L* is brightness, a* and b* are colors. Experimental results show that compared with the existing titanium-containing pearlescent pigments, the L, a, and b data of the titanium-free silver white pearlescent pigment of the present invention are not much different, and have a better pearlescent effect.

[0177] The pearlescent pigment powders of Examples 1-14 and Comparative Examples 1-5 were sent to SGS for testing and evaluation of heavy metals, SPF values ​​and UVA PF values. The specific test results are shown in Table 3:

[0178] Table 3: Comparison of SPF value and UVA PF value results:

[0179]

[0180]

[0181] It can be seen that the SPF values ​​and UVA PF values ​​of Examples 1-11 are larger than those of Comparative Example 5, with the SPF values ​​increasing by about 10% to 30% year-on-year, and the UVA PF values ​​increasing by about 20% to 45% year-on-year, which is a large increase.

[0182] Table 4 is SGS heavy metal detection data (Example 1)

[0183]

[0184] In summary, the titanium-free silver-white pearlescent pigment of the present invention has passed the heavy metal detection. Compared with the mica titanium pearlescent pigment, it has good UV resistance, and the SPF value and UVA PF value are both large. The SPF value is increased by 10% to 30% compared with the mica titanium pearlescent pigment, and the UVA PF value is increased by 20% to 45% compared with the mica titanium pearlescent pigment, which is a large range. It can effectively alleviate the common color change and color migration phenomena of pearlescent pigments in the production and application process; and the skin feel is softer and smoother, not rough, and does not show paleness.

Claims

1. A titanium-free silver-white pearlescent pigment, characterized in that: The pearlescent pigment comprises: a substrate, a magnesium oxide layer coated and deposited on the surface of the substrate, a high refractive index layer coated and deposited on the surface of the magnesium oxide layer, and a protective layer coated and deposited on the surface of the high refractive index layer; The substrate is one of mica, glass flakes, SiO2 flakes, Al2O3 flakes and bismuth oxychloride; the high refractive index layer is a metal oxide layer with a refractive index greater than 1.8, and the metal oxide is one of ZrO2, CeO2, and ZnO; the protective layer is one or more of SiO2, Al2O3, and silane compounds; The coverage rate of the magnesium oxide layer is 0.2-6%, the coverage rate of the high refractive index layer is 10-45%, and the coverage rate of the protective layer is 0.05-7%.

2. The pearlescent pigment according to claim 1, characterized in that: The substrate is one of mica flakes, glass flakes, SiO2 flakes, Al2O3 flakes and bismuth oxychloride flakes; and / or The metal oxide is CeO2 and / or ZnO; and / or The protective layer is SiO2 and / or Al2O3; and / or The protective layer is a silane compound, and the silane compound is selected from one or more of (3-glycidyloxypropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane, methacrylpropylmethoxysilane, 3-(2-aminoethylamino)propyltrimethoxysilane, methyltriethoxysilane, and n-hexyltrimethoxysilane.

3. The pearlescent pigment according to claim 2, characterized in that: The protective layer is SiO2.

4. The pearlescent pigment according to any one of claims 1 to 3, characterized in that: The coverage rate of the magnesium oxide layer is 0.5-5%; and / or The coverage of the high refractive index layer is 15-40%; and / or The coverage of the protective layer is 0.1-6%.

5. The pearlescent pigment according to claim 4, characterized in that: The coverage rate of the magnesium oxide layer is 1-4%; and / or The coverage of the high refractive index layer is 20-35%; and / or The coverage rate of the protective layer is 0.3-5%.

6. The pearlescent pigment according to any one of claims 1 to 3 and 5, characterized in that: The thickness of the substrate is 50-500nm; the particle size of the substrate is ≤500μm.

7. The pearlescent pigment according to claim 4, characterized in that: The thickness of the substrate is 50-500nm; the particle size of the substrate is ≤500μm.

8. The pearlescent pigment according to claim 6, characterized in that: The thickness of the substrate is 75-450 nm; the particle size of the substrate is ≤300 μm.

9. The pearlescent pigment according to claim 7, characterized in that: The thickness of the substrate is 75-450 nm; the particle size of the substrate is ≤300 μm.

10. The pearlescent pigment according to claim 8 or 9, characterized in that: The thickness of the substrate is 100-400 nm; the particle size of the substrate is ≤250 μm.

11. A method for preparing the titanium-free silver-white pearlescent pigment according to any one of claims 1 to 10, characterized in that: The preparation method comprises: 1) dispersing the substrate in the dispersion to obtain a first suspension; 2) adding a soluble magnesium salt solution to the first suspension to obtain a second suspension; 3) adding a soluble metal salt solution to the second suspension to obtain a third suspension; 4) adding a soluble protective salt solution to the third suspension to obtain a fourth suspension; 5) The fourth suspension is filtered, washed, dried, calcined and sieved in sequence to obtain a titanium-free silver-white pearlescent pigment.

12. The method according to claim 11, characterized in that: The dispersion liquid is deionized water, and the liquid-to-solid mass ratio of the dispersion liquid to the added amount of the substrate is 3-20:1; and / or The soluble magnesium salt is one or more of magnesium nitrate, magnesium sulfate, and magnesium chloride; the concentration of the soluble magnesium salt solution is 25-600 g / L; the amount of the soluble magnesium salt solution added is such that the coverage rate of the soluble magnesium salt in the second suspension on the substrate surface is 0.5-15%.

13. The method according to claim 12, characterized in that: The liquid-to-solid mass ratio of the dispersion to the added amount of the substrate is 5-15:1; and / or The concentration of the soluble magnesium salt solution is 50-300 g / L; the amount of the soluble magnesium salt solution added is such that the coverage rate of the soluble magnesium salt in the second suspension on the surface of the substrate is 0.8-12%.

14. The method according to claim 13, characterized in that: The liquid-to-solid mass ratio of the dispersion to the added amount of the substrate is 7-12:1; and / or The concentration of the soluble magnesium salt solution is 80-200 g / L; the amount of the soluble magnesium salt solution added is such that the coverage rate of the soluble magnesium salt in the second suspension on the surface of the substrate is 1-10%.

15. The method according to any one of claims 11 to 14, characterized in that: The soluble metal salt is one or more of cerium nitrate, cerium chloride, cerium sulfate, zinc nitrate, zinc sulfate, and zinc chloride; the concentration of the soluble metal salt solution is 80-700 g / L; the amount of the soluble metal salt solution added is such that the coverage rate of the soluble metal salt in the third suspension is 25-88%.

16. The method according to claim 15, characterized in that: The soluble metal salt is a mixed salt of one or more of cerium nitrate, cerium chloride, cerium sulfate and one or more of zinc nitrate, zinc sulfate, zinc chloride; the concentration of the soluble metal salt solution is 100-500g / L; the amount of the soluble metal salt solution added is such that the coverage rate of the soluble metal salt in the third suspension is 30-80%.

17. The method according to claim 16, characterized in that: The soluble metal salt is a mixed salt of cerium nitrate and zinc chloride; the concentration of the soluble metal salt solution is 120-300 g / L; the amount of the soluble metal salt solution added is such that the coverage rate of the soluble metal salt in the third suspension is 35-75%.

18. The method according to any one of claims 11-14, 16-17, characterized in that: The soluble protective salt is one or more of aluminum chloride, aluminum nitrate, aluminum sulfate, sodium metasilicate pentahydrate, sodium metasilicate nonahydrate, and silane compounds; the concentration of the soluble protective salt solution is 30-250 g / L; the amount of the soluble protective salt solution added is such that the coverage rate of the soluble protective salt in the fourth suspension is 0.1-20%.

19. The method according to claim 18, characterized in that: The soluble protective salt is aluminum chloride and / or sodium metasilicate pentahydrate; the concentration of the soluble protective salt solution is 40-200 g / L; the amount of the soluble protective salt solution added is such that the coverage rate of the soluble protective salt in the fourth suspension is 0.5-15%.

20. The method according to claim 19, characterized in that: The soluble protective salt is sodium metasilicate pentahydrate; the concentration of the soluble protective salt solution is 50-180 g / L; the amount of the soluble protective salt solution added is such that the coverage rate of the soluble protective salt in the fourth suspension is 0.8-10%.

21. The method according to claim 18, characterized in that: Step 1) is specifically as follows: dispersing the substrate in the dispersion in proportion, stirring and mixing thoroughly, heating to a constant temperature of 50-90° C., and adjusting the pH of the system to 7-9 with an acid or alkali to obtain a first suspension; and / or Step 2) is specifically: adding a soluble magnesium salt solution to the first suspension in proportion, controlling the temperature to 65-90° C., and adjusting the pH of the system to 7-9 with an acid or base to obtain a second suspension; and / or Step 3) is specifically: adding a soluble metal salt solution to the second suspension in proportion, controlling the temperature to 65-90° C., and adjusting the pH of the system to 5-9 with an acid or base to obtain a third suspension; and / or Step 4) is specifically as follows: adding a soluble protective salt solution to the third suspension in proportion, controlling the temperature to 65-90° C., and adjusting the pH of the system to 7-10 with an acid or base to obtain a fourth suspension; Step 5) is specifically as follows: the fourth suspension is filtered, washed, and then dried in an oven at 80-150°C. After drying, it is calcined at 700-900°C for 1-15 minutes and sieved to obtain a titanium-free silver white pearlescent pigment.

22. The method according to claim 21, characterized in that: Step 1) is specifically as follows: dispersing the substrate in the dispersion in proportion, stirring and mixing thoroughly, heating to a constant temperature of 75-85° C., and adjusting the pH of the system to 7.5-8.5 with a hydrochloric acid solution with a mass concentration of 5-18% or a sodium hydroxide solution with a mass concentration of 5-15% to obtain a first suspension; and / or Step 2) is specifically: adding a soluble magnesium salt solution to the first suspension in proportion, controlling the temperature to 75-85° C., and adjusting the pH of the system to 7.5-8.5 with a hydrochloric acid solution with a mass concentration of 5-18% or a sodium hydroxide solution with a mass concentration of 5-15% to obtain a second suspension; and / or Step 3) is specifically: adding a soluble metal salt solution to the second suspension in proportion, controlling the temperature to 75-85° C., and adjusting the pH of the system to 5.5-8.5 with a hydrochloric acid solution with a mass concentration of 5-18% or a sodium hydroxide solution with a mass concentration of 5-15% to obtain a third suspension; and / or Step 4) is specifically as follows: adding a soluble protective salt solution to the third suspension in proportion, controlling the temperature to 75-85° C., and adjusting the pH of the system to 7.5-9 with a hydrochloric acid solution with a mass concentration of 5-18% or a sodium hydroxide solution with a mass concentration of 5-15% to obtain a fourth suspension; Step 5) is specifically as follows: the fourth suspension is filtered, washed, and then dried in an oven at 100-135°C. After drying, it is calcined at 750-850°C for 2-10 minutes and sieved to obtain a titanium-free silver white pearlescent pigment.

23. Use of the titanium-free silver white pearlescent pigment according to any one of claims 1 to 10, characterized in that: The titanium-free silver white pearlescent pigment is used to prepare one or more of coatings, inks, plastics and cosmetics.

24. The use according to claim 23, characterized in that: The titanium-free silver-white pearlescent pigment is used to prepare one or more of lip gloss, eye shadow, pressed powder, nail polish, body lotion, face cream, shampoo, facial cleanser and handmade soap.

Citation Information

Patent Citations

  • Preparation method of super-large-particle-size synthetic-substrate pearlescent pigment

    CN106833030A

  • Angle-different color pearlescent pigment

    CN107434924A

  • Rutile type interference color pearlescent pigment with high color saturation degree and preparation method thereof

    CN108084743A

  • Preparation method of titanium dioxide pigment

    CN111777876A

  • Titanium-free golden pearlescent pigment as well as preparation method and application thereof

    CN114276700A