A high weather resistance APP modified asphalt waterproofing membrane and preparation method thereof

By adding polyester non-woven fabric and styrene-butadiene rubber powder during the preparation process of the modified asphalt waterproofing membrane, and using silver ion antibacterial additives, the deficiencies of the modified asphalt waterproofing membrane in terms of strength, durability and antibacterial properties are solved , achieving higher waterproof performance and long-lasting use.

CN117656607BActive Publication Date: 2024-10-01NANTONG RUIRUI WATERPROOF NEW TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311681077.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-08
Publication Date
2024-10-01
Estimated Expiration
2043-12-08

AI Technical Summary

Technical Problem

Existing modified asphalt waterproofing membranes have deficiencies in strength, durability, flexibility, bonding performance and antibacterial properties, and cannot effectively improve their lasting use.

Method used

By adding polyester non-woven fabric, styrene-butadiene rubber powder and silver ion antibacterial additives during the preparation process, and using heating stirring and spraying technology, a uniform composite system and antibacterial layer are formed to enhance the strength, durability and antibacterial performance of asphalt.

Benefits of technology

Significantly improves the strength, durability, flexibility and antibacterial properties of the modified asphalt waterproofing membrane, ensuring its long-lasting use under different environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117656607B_ABST
    Figure CN117656607B_ABST
Patent Text Reader

Abstract

The invention discloses a highly weather-resistant APP modified asphalt waterproofing coiled material and a preparation method thereof, and relates to the technical field of modified asphalt waterproofing coiled materials, including raw material preparation, wherein the raw materials need to be mixed and processed after the raw materials are prepared, and the mixing and processing need to fill the asphalt. The invention obtains dry and pollution-free polyester non-woven fabric through polyester non-woven fabric, gradually adds the polyester non-woven fabric into the heated modified polypropylene asphalt by heating with a heating boiler, stirs the polyester non-woven fabric and the asphalt with a stirrer, pours the asphalt mixture into an iron container, and puts the iron container containing the asphalt mixture into a heating oven, ensuring that the polyester non-woven fabric is fully dispersed in the modified polypropylene asphalt, thereby helping to ensure that the performance of the mixture is evenly distributed, thereby being able to increase the strength and durability of the highly weather-resistant APP modified asphalt waterproofing coiled material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of modified asphalt waterproofing coiled materials, in particular to a highly weather-resistant APP modified asphalt waterproofing coiled material and a preparation method thereof. Background Art

[0002] Modified asphalt waterproofing membrane is one of the indispensable materials in rooftop construction work. By sticking highly weather-resistant APP modified asphalt waterproofing membrane on the roof of the building, it can provide a waterproofing function for the roof of the building. At the same time, the APP modified asphalt waterproofing membrane has a high weather resistance function, and the material can be used for a long time. The highly weather-resistant APP modified asphalt waterproofing membrane and the preparation method provided by the present invention can improve the strength and durability of the modified asphalt waterproofing membrane through fillers, enhance the flexibility of modified polypropylene asphalt through additives, and improve its bonding performance. Through reasonable coating, the performance and weather resistance of the modified asphalt waterproofing membrane can be increased, and by adding a bactericide, the antibacterial property of the modified asphalt waterproofing membrane is improved, thereby improving the long-term use of the modified asphalt waterproofing membrane.

[0003] The defects of existing modified asphalt waterproof membranes are:

[0004] 1. The application document JP2003027021A discloses a recyclable modified asphalt waterproofing membrane, which mainly considers the production of a recyclable modified asphalt waterproofing sheet that can be recycled after use and reused as a raw material for a self-adhesive layer, but does not consider how to improve the strength and durability of the modified asphalt waterproofing membrane;

[0005] 2. Application document KR1020090030804A discloses polymer modified asphalt waterproofing membrane, which mainly considers the improvement of construction quality, but does not consider how to enhance the flexibility of modified polypropylene asphalt and improve its bonding performance;

[0006] 3. Application document US20100316866A1 discloses a polymer modified asphalt waterproofing membrane containing aluminum silicate microbeads, which mainly considers reducing the weight of waterproof membranes used in the construction industry and improving the performance of waterproof membranes, but does not consider how to increase the performance and weather resistance of the modified asphalt waterproofing membrane;

[0007] 4. Patent document CN103802380B discloses a modified asphalt waterproofing membrane, which mainly considers high dimensional stability, convenient construction, reliable bonding, and self-healing properties. It does not consider how to improve the antibacterial properties of the modified asphalt waterproofing membrane, thereby improving the long-term use of the modified asphalt waterproofing membrane. Summary of the invention

[0008] The object of the present invention is to provide a highly weather-resistant APP modified asphalt waterproofing membrane and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0009] To achieve the above object, the present invention provides the following technical solutions: a highly weather-resistant APP modified asphalt waterproofing coiled material and a preparation method thereof, comprising raw material preparation, the raw materials need to be mixed and processed after the raw materials are prepared, and the mixing and processing require filling work on the asphalt;

[0010] The filler is prepared by gradually adding polyester non-woven fabric into asphalt, controlling the amount of polyester non-woven fabric added, and the ratio of asphalt to polyester non-woven fabric is 92:8. A mixer is used to stir the polyester non-woven fabric and asphalt, the stirring speed is set to 180 rpm, the stirring time is set to 3 minutes, the asphalt mixture is poured into an iron container, and the iron container containing the asphalt mixture is placed in a heating oven, the heating oven temperature is set to 160°C, and the heating time is five hours.

[0011] Preferably, the method for preparing the highly weather-resistant APP modified asphalt waterproofing membrane comprises the following steps:

[0012] Step S1, raw material preparation: select modified polypropylene asphalt and polypropylene film.

[0013] Preferably, the method for preparing the highly weather-resistant APP modified asphalt waterproofing membrane further comprises the following steps:

[0014] Step S2, mixing and processing: adding fillers and additives to the modified polypropylene asphalt, and heating and stirring the mixed modified polypropylene asphalt;

[0015] Step S21: Before adding the polyester non-woven fabric to the modified polypropylene asphalt, cut the polyester non-woven fabric into square sheets with a length of 0.5 cm, move the solidified modified polypropylene asphalt into a heating boiler, set the temperature of the heating boiler to 150°C, and wait until the modified polypropylene asphalt in the heating boiler flows.

[0016] Step S22, by using a heating boiler, set the heating temperature to 150°C, heat the modified polypropylene asphalt again to make it flow, add styrene-butadiene rubber powder to the modified polypropylene asphalt in a ratio of 10:90, continue to heat the polypropylene asphalt and the modified styrene-butadiene rubber together, set the stirring speed of the mixer to 180 rpm, set the stirring time to 3 minutes, use the mixer to mix the polypropylene asphalt and the modified styrene-butadiene rubber, and after the mixing is completed, put the mixture into a cooling box, and set the temperature in the cooling box to 20°C.

[0017] Preferably, the method for preparing the highly weather-resistant APP modified asphalt waterproofing membrane further comprises the following steps:

[0018] Step S3, coating: setting the temperature of the heating boiler to 150° C. to heat and flow the mixture, and coating the mixture onto the polypropylene film;

[0019] Use a soft brush, sponge and air gun with water and detergent to clean the surface of the polypropylene film substrate in advance, use another clean soft brush, dip it in the solution containing epoxy silane, and brush the polypropylene film substrate with the soft brush, and stick the glass fiber grid on the top of the polypropylene film substrate. While the polypropylene film substrate is standing, set the heating boiler temperature to 150°C to heat and flow the mixture, and then use a mixer to stir the mixture, pour the mixture into the sprayer, set the spraying pressure of the sprayer to 18MPa, and the spraying speed to between 0.24km and 0.26km / h, spray the mixture on the top of the glass fiber grid with the sprayer, and sprinkle quartz sand particles on the mixture.

[0020] Preferably, the method for preparing the highly weather-resistant APP modified asphalt waterproofing membrane further comprises the following steps:

[0021] Step S4, curing and treating: curing and treating the applied mixture coating;

[0022] After coating is completed, the coated mixture is placed in a drying oven, the temperature of the drying oven is set to 80° C., and the mixture coating is dried.

[0023] Preferably, the method for preparing the highly weather-resistant APP modified asphalt waterproofing membrane further comprises the following steps:

[0024] Step S5, testing and quality control: testing the prepared high weather resistance APP modified asphalt waterproof membrane;

[0025] After the mixture is dried, the coating is inspected and tested;

[0026] Coating Inspection and Testing:

[0027] (1) Thickness measurement;

[0028] (2) Adhesion test;

[0029] (3) Hardness test;

[0030] (4) Corrosion resistance test;

[0031] (5) Appearance inspection;

[0032] (6) Chemical performance test;

[0033] (7) Weather resistance test.

[0034] Preferably, the method for preparing the highly weather-resistant APP modified asphalt waterproofing membrane further comprises the following steps:

[0035] Step S6, applying an antibacterial additive;

[0036] After testing the high weather resistance APP modified asphalt waterproofing membrane, select silver ion antibacterial additives, pour the silver ion antibacterial additives into the sprayer, set the spraying pressure of the sprayer to 12MPa, the spraying speed to between 0.2 km and 0.24 km / h, and the spraying distance to 0.4 meters. After spraying, let the high weather resistance APP modified asphalt waterproofing membrane stand for 20 minutes, and send the sprayed modified polypropylene asphalt waterproofing membrane into the oven, set the oven temperature to 60°C, and set the oven drying time to 30 minutes. After the drying work is completed, the antibacterial properties of the high weather resistance APP modified asphalt waterproofing membrane are verified.

[0037] Preferably, the method for preparing the highly weather-resistant APP modified asphalt waterproofing membrane further comprises the following steps:

[0038] Step S61, observing the microstructure of the surface of the modified asphalt waterproof membrane through a scanning electron microscope.

[0039] Preferably, it includes a protective layer, a surface coating, a modified asphalt layer, a reinforcing layer, a supporting layer and a back coating, the protective layer is a silver ion antibacterial additive layer, the surface coating is a quartz sand particle layer, the modified asphalt layer is a polypropylene modified asphalt mixed layer, the reinforcing layer is a glass fiber mesh layer, the supporting layer is a polypropylene film substrate, the back coating is an epoxy silane solution layer, the reinforcing layer is adhered to the top of the supporting layer through an epoxy silane solution, the top of the reinforcing layer is sprayed with a modified asphalt layer, the top of the modified asphalt layer is adhered with a surface coating through an epoxy silane solution, the top of the surface coating is sprayed with a protective layer, and the bottom of the supporting layer is coated with a back coating.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] 1. The present invention obtains dry and pollution-free polyester non-woven fabric through polyester non-woven fabric, heats it to 150°C by using a heating boiler to make it sufficiently fluid, and at the same time, cuts the polyester non-woven fabric into square sheets with a length of 0.5 cm, gradually adds the polyester non-woven fabric into the heated modified polypropylene asphalt, uses a mixer to stir the polyester non-woven fabric and the asphalt to ensure that the polyester non-woven fabric is evenly dispersed in the asphalt, continues to stir and maintain an appropriate temperature to ensure that the polyester non-woven fabric is fully mixed with the asphalt, thereby helping to ensure that the polyester non-woven fabric and the asphalt form a uniform composite system, pours the asphalt mixture into an iron container, and puts the iron container containing the asphalt mixture into a heating oven to ensure that the polyester non-woven fabric is fully dispersed in the modified polypropylene asphalt, thereby helping to ensure that the performance of the mixture is evenly distributed, thereby increasing the strength and durability of the high weather-resistant APP modified asphalt waterproof membrane.

[0042] 2. The present invention heats the modified polypropylene asphalt again by using a heating boiler to make it flow, adds styrene-butadiene rubber powder to the modified polypropylene asphalt, continues to heat the polypropylene asphalt and the modified styrene-butadiene rubber together to ensure that the styrene-butadiene rubber is fully dispersed in the asphalt, mixes the polypropylene asphalt and the modified styrene-butadiene rubber by using a stirrer to ensure that the modified styrene-butadiene rubber fully interacts with the polypropylene asphalt, and after the mixing is completed, puts the mixture into a cooling box to prevent quality changes, thereby enhancing the flexibility of the modified polypropylene asphalt and improving its bonding performance.

[0043] 3. The present invention is coated. Before coating, water is poured on the substrate of the polypropylene film, and then a neutral detergent is dripped onto the substrate of the polypropylene film stained with water, and the polypropylene film is cleaned with a soft brush. At the same time, a mild and moist sponge is used to wipe the surface of the polypropylene film, and then an air blow gun is used to remove dust and impurities on the polypropylene film. Another clean soft brush is dipped in a solution containing epoxy silane, and the substrate of the polypropylene film is brushed with the soft brush. A glass fiber grid is pasted on the top of the substrate of the polypropylene film. During the static state of the substrate of the polypropylene film, a heating boiler is set to heat and flow the mixture, and then a mixer is used to stir the mixture, and the mixture is poured into a sprayer, and the mixture is sprayed on the top of the glass fiber grid by the sprayer to ensure that the thickness of the coated mixture is uniform, and quartz sand particles are sprinkled on the mixture, thereby increasing the performance and weather resistance of the modified asphalt waterproof membrane.

[0044] 4. The present invention selects a silver ion antibacterial additive after testing the high-weather-resistant APP modified asphalt waterproofing membrane, pre-treats the silver ion antibacterial additive to ensure that it can be evenly dispersed in the polypropylene asphalt, pours the silver ion antibacterial additive into a sprayer, thereby ensuring that the silver ion antibacterial additive can be evenly covered on the surface of the polypropylene asphalt waterproofing membrane. After spraying, the sprayed modified polypropylene asphalt waterproofing membrane is sent into an oven. The polypropylene asphalt waterproofing membrane needs to be cured so that the silver ion antibacterial additive can be firmly attached to the surface and ensure that the antibacterial effect is long-lasting and stable. After the drying work is completed, the antibacterial property of the high-weather-resistant APP modified asphalt waterproofing membrane is verified, the microstructure of the surface of the modified asphalt waterproofing membrane is observed by a scanning electron microscope, and the distribution of the added antibacterial agent on the surface is analyzed. The waterproofing membrane that passes the test is packaged and stored under dry conditions to ensure that the product quality is not affected, thereby improving the antibacterial property of the modified asphalt waterproofing membrane, thereby improving the long-lasting use of the modified asphalt waterproofing membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 is an axonometric view of the present invention;

[0046] Figure 2 This is a flow chart of the modified asphalt waterproofing membrane of the present invention;

[0047] Figure 3 A detailed diagram of the testing and quality control classification of the present invention. DETAILED DESCRIPTION

[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0049] See also Figure 1 and Figure 2, a highly weather-resistant APP modified asphalt waterproofing coiled material and a preparation method thereof, comprising a protective layer, a protective layer 1, a surface coating 2, a modified asphalt layer 3, a reinforcing layer 4, a supporting layer 5 and a back coating 6, wherein the protective layer 1 is a silver ion antibacterial additive layer, the surface coating 2 is a quartz sand particle layer, the modified asphalt layer 3 is a polypropylene modified asphalt mixed layer, the reinforcing layer 4 is a glass fiber mesh layer, the supporting layer 5 is a substrate of a polypropylene film, the back coating 6 is an epoxy silane solution layer, the top of the supporting layer 5 is adhered with the reinforcing layer 4 through an epoxy silane solution, the top of the reinforcing layer 4 is sprayed with the modified asphalt layer 3, the top of the modified asphalt layer 3 is adhered with the surface coating 2 through an epoxy silane solution, the top of the surface coating 2 is sprayed with the protective layer 1, and the bottom of the supporting layer 5 is coated with the back coating 6;

[0050] Step S1, raw material preparation: selecting modified polypropylene asphalt and polypropylene film;

[0051] The surface coating 2 is located at the outermost layer of the waterproof membrane and is responsible for direct contact with the external environment. A protective layer 1 is added on the surface coating 2 to enhance the wear resistance and scratch resistance of the waterproof membrane. The modified asphalt layer 3 contains asphalt, APP, polyester non-woven fabric and styrene-butadiene rubber powder. The addition of APP can improve the flexibility, cold resistance and weather resistance of asphalt. The addition of polyester non-woven fabric can increase the strength and durability of high weather resistance APP modified asphalt waterproof membrane. The addition of styrene-butadiene rubber powder can enhance the flexibility of modified polypropylene asphalt and improve its bonding performance. The reinforcement layer 4 is located below the modified asphalt layer and is used to enhance the mechanical properties of the waterproof membrane. A support layer 5 is added below the reinforcement layer 4 to enhance the stability of the overall structure. The back coating 6 is located at the bottom layer of the waterproof membrane and can improve the adhesion of the substrate and provide further waterproof protection. Example

[0052] See also Figure 1 and Figure 2 , a highly weather-resistant APP modified asphalt waterproofing membrane and a preparation method thereof, comprising step S2, mixing and processing: adding filler to modified polypropylene asphalt, and heating and stirring the mixed modified polypropylene asphalt;

[0053] Step S21, before adding the polyester non-woven fabric to the modified polypropylene asphalt, cut the polyester non-woven fabric into square sheets with a length of 0.5 cm, move the solidified modified polypropylene asphalt to the heating boiler, set the temperature of the heating boiler to 150°C, until the modified polypropylene asphalt in the heating boiler flows, and the raw materials need to be mixed and processed after preparation, and the mixing and processing require filling of the asphalt; the filler is when preparing the asphalt, gradually add the polyester non-woven fabric to the asphalt, control the addition amount of the polyester non-woven fabric, the ratio of asphalt to polyester non-woven fabric is 92:8, use a stirrer to stir the polyester non-woven fabric and the asphalt, set the stirring speed to 180 rpm, set the stirring time to 3 minutes, pour the asphalt mixture into an iron container, put the iron container containing the asphalt mixture into a heating oven, set the heating oven temperature to 160°C, and the heating time to five hours;

[0054] Obtain dry and pollution-free polyester non-woven fabric. Odor and steam will be generated during the processing, so choose a ventilated workplace. Heat the modified polypropylene asphalt to 150°C by using a heating boiler to make it sufficiently fluid. At the same time, cut the polyester non-woven fabric into square sheets with a length of 0.5 cm. Gradually add the polyester non-woven fabric to the heated modified polypropylene asphalt. Control the amount of polyester non-woven fabric added. The ratio of asphalt to polyester non-woven fabric is 92:8. Use a mixer to stir the polyester non-woven fabric and asphalt. The stirring speed is set to 180 rpm and the stirring time is set to 3 minutes to ensure that the polyester non-woven fabric Evenly dispersed in the asphalt, continuously stirring and maintaining the appropriate temperature to ensure that the polyester non-woven fabric is fully mixed with the asphalt, thereby helping to ensure that the polyester non-woven fabric and the asphalt form a uniform composite system, pour the asphalt mixture into an iron container, put the iron container containing the asphalt mixture into a heating oven, set the heating oven temperature to 160°C, the heating time is five hours, and continuously stir and mix to ensure that the polyester non-woven fabric is fully dispersed in the modified polypropylene asphalt, thereby helping to ensure that the properties of the mixture are evenly distributed, and at the end of the production stage, physical property tests and viscosity tests are performed to ensure that the performance of the modified polypropylene asphalt meets expectations;

[0055] The tensile strength of the mixture is evaluated through tensile tests, the tear strength of the mixture is tested to evaluate its performance when subjected to tear stress, and the stability of the mixture under high temperature conditions is tested to understand its state in a high temperature environment. The rotational viscosity test is used to determine the viscosity of the mixture at different temperatures to understand its fluidity, and to evaluate the temperature sensitivity of the mixture, that is, how its viscosity changes with temperature, thereby increasing the strength and durability of the high weather-resistant APP modified asphalt waterproof membrane. Example

[0056] See also Figure 1 and Figure 2, a highly weather-resistant APP modified asphalt waterproofing membrane and a preparation method thereof, comprising step S2, mixing and processing: adding additives to modified polypropylene asphalt, and heating and stirring the mixed modified polypropylene asphalt;

[0057] Step S22, by using a heating boiler, setting the heating temperature to 150° C., heating the modified polypropylene asphalt again to make it flow, adding styrene-butadiene rubber powder to the modified polypropylene asphalt in a ratio of 10:90, continuing to heat the polypropylene asphalt and the modified styrene-butadiene rubber together, setting the stirring speed of the stirrer to 180 rpm, setting the stirring time to 3 minutes, and mixing the polypropylene asphalt and the modified styrene-butadiene rubber by using a stirrer. After the mixing is completed, put the mixture into a cooling box, and set the temperature in the cooling box to 20° C.;

[0058] By using a heating boiler, setting the heating temperature to 150°C, the modified polypropylene asphalt is heated again to make it flow, and the styrene-butadiene rubber powder is added to the modified polypropylene asphalt in a ratio of 10:90. The polypropylene asphalt and the modified styrene-butadiene rubber are continued to be heated together to reach a temperature of 150°C to ensure that the styrene-butadiene rubber is fully dispersed in the asphalt. The stirring speed of the mixer is set to 180 rpm and the stirring time is set to 3 minutes. The polypropylene asphalt and the modified styrene-butadiene rubber are mixed by using a mixer to ensure that the modified styrene-butadiene rubber fully interacts with the polypropylene asphalt. After the mixing is completed, the mixture is placed in a cooling box and the temperature in the cooling box is set to 20°C to prevent quality changes, thereby enhancing the flexibility of the modified polypropylene asphalt and improving its bonding properties. Example

[0059] See also Figure 1 and Figure 2 , a highly weather-resistant APP modified asphalt waterproofing membrane and a preparation method thereof, comprising step S3, coating: setting the heating boiler temperature to 150° C. to heat and flow the mixture, and coating the mixture on a polypropylene film;

[0060] Use a soft brush, sponge and air gun with water and detergent to clean the surface of the polypropylene film substrate in advance, use another clean soft brush to dip the solution containing epoxy silane, and use the soft brush to brush the polypropylene film substrate, paste the glass fiber mesh on the top of the polypropylene film substrate, set the heating boiler temperature to 150°C to heat and flow the mixture while the polypropylene film substrate is standing, and then use a mixer to stir the mixture, pour the mixture into the sprayer, set the spraying pressure of the sprayer to 18MPa, and the spraying speed to between 0.24km and 0.26km / h, spray the mixture on the top of the glass fiber mesh through the sprayer, and sprinkle quartz sand particles on the mixture;

[0061] Before coating, pour water on the substrate of the polypropylene film, then drop neutral detergent on the substrate of the polypropylene film stained with water, use a soft brush to clean the polypropylene film, and at the same time, use a mild and moist sponge to wipe the surface of the polypropylene film, and then use an air blow gun to remove dust and impurities from the polypropylene film. Use another clean soft brush, dip it in a solution containing epoxy silane, and use the soft brush to brush the substrate of the polypropylene film. Paste the glass fiber grid on the top of the substrate of the polypropylene film. While the substrate of the polypropylene film is standing, set the heating boiler temperature to 150°C to heat and flow the mixture, then use a mixer to stir the mixture, pour the mixture into the sprayer, set the spraying pressure of the sprayer to 18MPa, and the spraying speed to between 0.24 km and 0.26 km / h. Spray the mixture on the top of the glass fiber grid through the sprayer to ensure that the thickness of the coated mixture is uniform, and sprinkle quartz sand particles on the mixture to increase the performance and weather resistance of the modified asphalt waterproof membrane. Example

[0062] See also Figure 1 and Figure 2 , a highly weather-resistant APP modified asphalt waterproofing membrane and a preparation method thereof, comprising step S4, curing and treating: curing and treating the coated mixture coating;

[0063] After coating, the coated mixture is placed in a drying oven, the temperature of the drying oven is set to 80°C, and the mixture coating is dried;

[0064] The coating mixture is dried and solidified by the drying work of the drying furnace, and the uniformity of the drying and solidification process can be ensured, thereby improving the quality of the mixture. Example

[0065] See also Figure 1 , Figure 2 and Figure 3 , a highly weather-resistant APP modified asphalt waterproofing membrane and a preparation method thereof, comprising step S5, testing and quality control: testing the prepared highly weather-resistant APP modified asphalt waterproofing membrane;

[0066] After the mixture is dried, the coating is inspected and tested, and the parameters of the coating process are recorded;

[0067] Coating Inspection and Testing:

[0068] (1) Thickness measurement: Coating thickness gauge is used to determine the thickness of the coating to ensure its protective performance and appearance;

[0069] (2) Adhesion test: The adhesion performance between the coating and the substrate is evaluated by using a tensile test. Strong adhesion is the key to ensure the long-term durability of the coating.

[0070] (3) Hardness test: Use Rockwell hardness tester to evaluate the hardness of the coating. Hardness test can provide information about the wear resistance and scratch resistance of the coating.

[0071] (4) Corrosion resistance test: Conduct a wet heat cycle test to evaluate the coating's resistance to corrosion;

[0072] (5) Appearance inspection: visually inspect the color, gloss and surface smoothness of the coating to ensure that the appearance of the coating meets the design requirements;

[0073] (6) Chemical performance test: Conduct heat resistance test;

[0074] (7) Weather resistance test: Weather resistance test is conducted to evaluate its performance under different climatic conditions. Example

[0075] See also Figure 1 and Figure 2 , a highly weather-resistant APP modified asphalt waterproofing membrane and a preparation method thereof, comprising step S6, applying an antibacterial additive;

[0076] After testing the high-weather-resistant APP modified asphalt waterproofing membrane, select the silver ion antibacterial additive, pour the silver ion antibacterial additive into the sprayer, set the spraying pressure of the sprayer to 12MPa, the spraying speed to between 0.2 km and 0.24 km / h, and the spraying distance to 0.4 meters. After the spraying is completed, let the high-weather-resistant APP modified asphalt waterproofing membrane stand for 20 minutes, send the sprayed modified polypropylene asphalt waterproofing membrane into the oven, set the oven temperature to 60°C, and set the oven drying time to 30 minutes. After the drying work is completed, verify the antibacterial properties of the high-weather-resistant APP modified asphalt waterproofing membrane;

[0077] Step S61, observing the microstructure of the surface of the modified asphalt waterproofing membrane by scanning electron microscopy, and analyzing the distribution of the added antibacterial agent on the surface;

[0078] After testing the high weather resistance APP modified asphalt waterproofing membrane, select the silver ion antibacterial additive, pre-treat the silver ion antibacterial additive to ensure that it can be evenly dispersed in the polypropylene asphalt, pour the silver ion antibacterial additive into the sprayer, set the spraying pressure of the sprayer to 12MPa, the spraying speed to 0.2 km to 0.24 km / h, and the spraying distance to 0.4 meters, so as to ensure that the silver ion antibacterial additive can be evenly covered on the surface of the polypropylene asphalt waterproofing membrane. After the spraying is completed, let the high weather resistance APP modified asphalt waterproofing membrane stand for 20 minutes, send the sprayed modified polypropylene asphalt waterproofing membrane into the oven, and set the oven temperature to 60℃, set the oven drying time to 30 minutes, the polypropylene asphalt waterproof membrane needs to be cured so that the silver ion antibacterial additive can be firmly attached to the surface and ensure that the antibacterial effect is long-lasting and stable. After the drying work is completed, the antibacterial property of the high weather-resistant APP modified asphalt waterproof membrane is verified, and the microstructure of the surface of the modified asphalt waterproof membrane is observed by scanning electron microscopy, and the distribution of the added antibacterial agent on the surface is analyzed. The qualified waterproof membrane is packaged and stored under dry conditions to ensure that the product quality is not affected, thereby improving the antibacterial property of the modified asphalt waterproof membrane and thus improving the long-lasting use of the modified asphalt waterproof membrane.

[0079] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a highly weather-resistant APP modified asphalt waterproofing membrane, characterized in that: Including raw material preparation, after which the raw materials need to be mixed and processed, and the mixing and processing require filling work on the asphalt; The filler work is to gradually add the polyester non-woven fabric into the asphalt during the preparation of the asphalt, control the amount of the polyester non-woven fabric added, and the ratio of the asphalt to the polyester non-woven fabric is 92:

8. A stirrer is used to stir the polyester non-woven fabric and the asphalt, and the stirring speed is set to 180 rpm and the stirring time is set to 3 minutes. The asphalt mixture is poured into an iron container, and the iron container containing the asphalt mixture is placed in a heating oven, and the temperature of the heating oven is set to 160° C. and the heating time is five hours. The method for preparing the highly weather-resistant APP modified asphalt waterproofing membrane comprises the following steps: Step S1, raw material preparation: selecting modified polypropylene asphalt and polypropylene film; Step S2, mixing and processing: adding fillers and additives to the modified polypropylene asphalt, and heating and stirring the mixed modified polypropylene asphalt; In step S2, the following steps are included: Step S21, before adding the polyester non-woven fabric to the modified polypropylene asphalt, cut the polyester non-woven fabric into square sheets with a length of 0.5 cm, move the solidified modified polypropylene asphalt to the heating boiler, set the temperature of the heating boiler to 150° C., until the modified polypropylene asphalt in the heating boiler flows, and then perform the filling work; Step S22, by using a heating boiler, setting the heating temperature to 150° C., heating the modified polypropylene asphalt again to make it flow, adding styrene-butadiene rubber powder to the modified polypropylene asphalt in a ratio of 10:90, continuing to heat the polypropylene asphalt and the modified styrene-butadiene rubber together, setting the stirring speed of the stirrer to 180 rpm, setting the stirring time to 3 minutes, and mixing the polypropylene asphalt and the modified styrene-butadiene rubber by using a stirrer. After the mixing is completed, put the mixture into a cooling box, and set the temperature in the cooling box to 20° C.; Step S3, coating: setting the temperature of the heating boiler to 150° C. to heat and flow the mixture, and coating the mixture onto the polypropylene film; Use a soft brush, sponge and air gun with water and detergent to clean the surface of the polypropylene film substrate in advance, use another clean soft brush to dip the solution containing epoxy silane, and use the soft brush to brush the polypropylene film substrate, paste the glass fiber mesh on the top of the polypropylene film substrate, set the heating boiler temperature to 150°C to heat and flow the mixture while the polypropylene film substrate is standing, and then use a mixer to stir the mixture, pour the mixture into the sprayer, set the spraying pressure of the sprayer to 18MPa, and the spraying speed to between 0.24km and 0.26km / h, spray the mixture on the top of the glass fiber mesh through the sprayer, and sprinkle quartz sand particles on the mixture; Step S4, curing and treating: curing and treating the applied mixture coating; After coating, the coated mixture is placed in a drying oven, the temperature of the drying oven is set to 80°C, and the mixture coating is dried; Step S5, testing and quality control: testing the prepared high weather resistance APP modified asphalt waterproof membrane; After the mixture is dried, the coating is inspected and tested; Coating Inspection and Testing: (1) Thickness measurement; (2) Adhesion test; (3) Hardness test; (4) Corrosion resistance test; (5) Appearance inspection; (6) Chemical performance test; (7) Weathering resistance test; Step S6, applying an antibacterial additive; After testing the high-weather-resistant APP modified asphalt waterproofing membrane, select the silver ion antibacterial additive, pour the silver ion antibacterial additive into the sprayer, set the spraying pressure of the sprayer to 12MPa, the spraying speed to between 0.2 km and 0.24 km / h, and the spraying distance to 0.4 meters. After the spraying is completed, let the high-weather-resistant APP modified asphalt waterproofing membrane stand for 20 minutes, send the sprayed modified polypropylene asphalt waterproofing membrane into the oven, set the oven temperature to 60°C, and set the oven drying time to 30 minutes. After the drying work is completed, verify the antibacterial properties of the high-weather-resistant APP modified asphalt waterproofing membrane; In step S6, the following steps are included: Step S61, observing the microstructure of the surface of the modified asphalt waterproof membrane through a scanning electron microscope.

2. A highly weather-resistant APP modified asphalt waterproofing membrane, using the method for preparing a highly weather-resistant APP modified asphalt waterproofing membrane according to claim 1, characterized in that: The invention comprises a protective layer (1), a surface coating (2), a modified asphalt layer (3), a reinforcing layer (4), a supporting layer (5) and a back coating (6), wherein the protective layer (1) is a silver ion antibacterial additive layer, the surface coating (2) is a quartz sand particle layer, the modified asphalt layer (3) is a polypropylene modified asphalt mixed layer, the reinforcing layer (4) is a glass fiber mesh layer, the supporting layer (5) is a polypropylene film substrate, the back coating (6) is an epoxy silane solution layer, the top of the supporting layer (5) is adhered to the reinforcing layer (4) by epoxy silane solution, the top of the reinforcing layer (4) is sprayed with the modified asphalt layer (3), the top of the modified asphalt layer (3) is adhered to the surface coating (2) by epoxy silane solution, the top of the surface coating (2) is sprayed with the protective layer (1), and the bottom of the supporting layer (5) is coated with the back coating (6).