Absorbable collagen hemostatic sponge and preparation method thereof
By using a combination of amino-modified polyglutamic acid, purified type I collagen and porous starch microspheres, a highly hygroscopic and flexible absorbable collagen hemostatic sponge was prepared, which solved the problem of the hemostatic effect of existing hemostatic materials during surgery. It achieves the effects of rapid hemostasis and wound healing by solving the problems of poor performance and poor degradation performance.
Patent Information
- Application Number
- CN202311731221.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-15
AI Technical Summary
Existing hemostatic materials have unsatisfactory hemostatic effects during surgery, especially for large-area open wounds and fragile vascular tissues. Traditional hemostatic materials have poor degradation properties and may cause secondary damage, and collagen hemostatic sponges are hygroscopic and Insufficient flexibility makes it difficult to stop bleeding quickly and effectively and promote healing.
An absorbable collagen hemostatic sponge including amino-modified polyglutamic acid, purified type I collagen and porous starch microspheres is used to improve the hygroscopicity, flexibility and biocompatibility of the sponge through specific raw material ratios and preparation methods. , enabling it to better adapt to wound shapes and changes, and promote wound healing.
It achieves efficient hygroscopicity and flexibility, can quickly adapt to the shape of the wound, improves the hemostatic effect and wound healing ability, and the preparation method is simple and suitable for mass production.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of hemostatic sponges, and in particular to an absorbable collagen hemostatic sponge and a preparation method thereof. Background Art
[0002] Surgical bleeding is one of the most common clinical manifestations after surgical trauma. Reducing surgical bleeding and shortening the operation time have an important impact on the patient's prognosis. In clinical surgery, for surgeries on solid organs such as the liver, spleen, brain, and kidneys, surgeries on fragile vascular lesions such as tumors, and other surgeries such as tooth extraction, as well as for patients with abnormal coagulation function, it is far from enough to rely solely on conventional methods such as electrocoagulation, compression, or suture to stop bleeding, and it must rely on the use of auxiliary hemostatic materials.
[0003] However, in the case of severe bleeding or massive bleeding from surgical wounds, the hemostatic effects of traditional hemostatic materials such as gauze, bandages, and cotton yarn are far from ideal. In addition, although the hemostatic effect of the new hemostatic sponge is better than that of traditional hemostatic materials, it has poor self-degradation performance and often causes unnecessary secondary damage to patients during the removal process.
[0004] In view of this situation, absorbable hemostatic materials have aroused widespread interest among scientific researchers. The use of absorbable hemostatic materials to treat bleeding during clinical surgery can achieve rapid local hemostasis, does not need to be removed, and can be degraded in the body, thus avoiding secondary damage caused by removing the dressing after hemostasis is completed.
[0005] Absorbable hemostatic materials mainly produce hemostatic effects by accelerating the blood coagulation process on the wound surface. Currently, the absorbable hemostatic products that are widely used in clinical practice include cellulose, starch and other plant polysaccharides, gelatin / collagen, chitosan, fibrinogen, etc. Different materials have different hemostatic mechanisms. Oxidized regenerated cellulose, starch, gelatin / collagen and chitosan hemostatic materials mainly form platelets by providing platelet activation and aggregation, and fibrinogen hemostatic materials can participate in the formation of fibrin clots in the coagulation cascade reaction.
[0006] However, existing hemostatic materials are treated / cross-linked with chemical additives, have a long degradation cycle, poor biomechanics, and the risk of chemical residues. Their cytotoxicity does not meet the standards, affecting wound healing. In addition, flocculent hemostatic materials have no fixed shape and are easy to fill, but they are in a loose and fragmented state and have poor adhesion to each other. When used to stop bleeding on large open beds, their blocking, filling and hemostatic effects are poor.
[0007] Compared with other hemostatic materials, collagen sponge has good hygroscopicity, biocompatibility and biodegradability, and collagen is also the most abundant protein in the human body, accounting for 25%-30% of the human body protein content. The porous collagen sponge has good water absorption performance and can absorb a large amount of water in the blood to form blood scabs to block blood vessels; at the same time, after vascular damage occurs, collagen can bind to platelet receptors, thereby promoting platelet adhesion and aggregation, and then starting the endogenous hemostatic mechanism. The organic combination of the two realizes the rapid hemostasis process of the wound. Studies have also shown that collagen can promote the migration of fibroblasts and macrophages, stimulate the regeneration of collagen in the body and the cleaning of cell fragments, thereby promoting tissue repair and healing. Collagen sponge can effectively promote wound healing while exerting good hemostatic properties. Therefore, it has good application prospects in clinical hemostasis.
[0008] However, the existing collagen hemostatic sponge has poor hygroscopicity, hard texture, poor ability to deform with the wound, and cannot completely match the wound during filling, which easily causes local over-filling or under-filling, fails to achieve the effect of rapid hemostasis, and is not conducive to wound healing.
[0009] Therefore, there is an urgent need to provide a hemostatic sponge with excellent hygroscopicity and excellent ability to deform with the wound. Summary of the invention
[0010] In order to solve at least one of the above technical problems, a hemostatic sponge with excellent hygroscopicity and excellent ability to deform with the wound is developed. The present application provides an absorbable collagen hemostatic sponge and a preparation method thereof.
[0011] In one aspect, the present application provides an absorbable collagen hemostatic sponge, comprising the following raw materials in parts by weight: 4.5-6.8 parts of amino-modified polyglutamic acid, 2.6-5.2 parts of purified type I collagen, 62-85 parts of acetic acid and 2.5-4 parts of porous starch microspheres;
[0012] The amino-modified polyglutamic acid is prepared from polyglutamic acid, ammonia water and ferric chloride in a weight ratio of 1:0.15-0.22:0.06-0.08.
[0013] By adopting the above technical solution, the hemostatic sponge prepared by the specific raw materials in the present application has excellent hygroscopicity and flexibility, and can better adapt to the shape and changes of the wound;
[0014] The specific purified type I collagen used in this application has excellent biocompatibility and the ability to promote cell attachment, which can promote wound healing;
[0015] The present application adopts a specific amino-modified polyglutamic acid to effectively improve the reactivity of polyglutamic acid, improve the water absorption, biocompatibility and degradation performance of polyglutamic acid, and help to improve the hemostatic effect and promote wound healing; at the same time, the amino-modified polyglutamic acid can also react with active groups such as hydroxyl and amino groups in type I collagen to improve the mechanical strength and stability of the hemostatic sponge;
[0016] The specific porous starch microspheres used in this application have excellent water absorption properties and good biocompatibility, which can be used as a carrier of the hemostatic sponge to provide better moisture absorption and air permeability; at the same time, the addition of porous starch microspheres can also improve the flexibility and deformability of the hemostatic sponge, enabling it to better adapt to the shape and changes of the wound.
[0017] Optionally, the amino-modified polyglutamic acid comprises 5-5.6 parts, purified type I collagen comprises 3.5-4.2 parts, acetic acid comprises 70-78 parts and porous starch microspheres comprises 3.2-3.5 parts.
[0018] By adopting the above technical solution, the present application uses a better range of raw materials, and the comprehensive performance of the prepared hemostatic sponge is more excellent.
[0019] Optionally, the specific surface area of the porous starch microspheres is 230-360 m 2 / g.
[0020] Optionally, the average particle size of the porous starch microspheres is 5-200 μm.
[0021] By adopting the above technical solution, the present application uses specific porous starch microspheres with a high specific surface area and good water absorption performance as a carrier to provide better moisture absorption and air permeability, while also effectively improving the flexibility and deformability of the hemostatic sponge.
[0022] Optionally, the porous starch microspheres are composed of porous starch microspheres with an average particle size of 5-80 μm and porous starch microspheres with an average particle size of 80-200 μm in a weight ratio of 1:0.5-0.8.
[0023] By adopting the above-mentioned technical scheme, the present application uses porous starch microspheres with different particle sizes to form a hemostatic sponge with different pore sizes but uniform distribution. At the same time, a better filling effect is formed in the internal structure of the hemostatic sponge, so that the porous starch microspheres with different particle sizes can complement each other, thereby improving the overall flexibility and hygroscopicity of the hemostatic sponge.
[0024] Optionally, the porous starch microspheres are mannitol-modified porous starch microspheres, which are prepared from porous starch microspheres, mannitol and sodium sulfate in a weight ratio of 1:0.3-0.5:0.08-0.12.
[0025] By adopting the above-mentioned technical scheme, the present application uses specific mannitol to modify the porous starch microspheres, so that the prepared hemostatic sponge has better hygroscopicity and flexibility, and can better adapt to the shape and changes of the wound; mannitol has good water absorption and flexibility. By combining mannitol with porous starch microspheres, the water absorption and flexibility of mannitol can be utilized to further improve the hygroscopicity and flexibility of the porous starch microspheres; at the same time, sodium sulfate can also promote blood coagulation and cell proliferation in the hemostatic process, thereby promoting wound healing.
[0026] Optionally, the concentration of the acetic acid is 0.03-0.06 mol / L.
[0027] On the other hand, the present application provides a method for preparing an absorbable collagen hemostatic sponge, comprising the following steps:
[0028] S1, dissolving amino-modified polyglutamic acid in 25-40 wt % acetic acid to prepare solution 1;
[0029] S2, dissolving purified type I collagen in 25-40 wt % acetic acid to prepare solution 2;
[0030] S3, dissolving the porous starch microspheres in the remaining acetic acid to prepare solution 3;
[0031] S4, mixing and stirring the solution 1, the solution 2 and the solution 3, and then homogenizing them to obtain a slurry;
[0032] S5. Pour the slurry into a mold and perform freeze-drying treatment to obtain the absorbable collagen hemostatic sponge.
[0033] By adopting the above technical scheme, the preparation method of the absorbable collagen hemostatic sponge of the present application is simple to operate and suitable for large-scale production. At the same time, hemostatic sponges of different thicknesses and shapes can be prepared according to different application scenarios, and the prepared absorbable collagen hemostatic sponge has excellent comprehensive performance.
[0034] Optionally, in S1, the method for preparing amino-modified polyglutamic acid comprises the following steps: dissolving polyglutamic acid in water, adding ammonia water and ferric chloride, mixing and stirring, and then purifying to prepare amino-modified polyglutamic acid.
[0035] By adopting the above technical scheme, the preparation method of amino-modified polyglutamic acid of the present application is simple to operate, and the prepared amino-modified polyglutamic acid effectively improves the reaction activity of polyglutamic acid, improves the water absorption, biocompatibility and degradation performance of polyglutamic acid, and helps to improve the hemostatic effect and promote wound healing.
[0036] Optionally, the mixing and stirring temperature is 30-40° C., and the mixing and stirring time is 1.5-2 h.
[0037] In summary, the present invention includes at least one of the following beneficial technical effects:
[0038] 1. The hemostatic sponge prepared by the specific raw materials in the present application has excellent hygroscopicity and flexibility, and can better adapt to the shape and changes of the wound;
[0039] 2. The present application adopts a specific amino-modified polyglutamic acid, which effectively improves the reactivity of polyglutamic acid and improves the water absorption of polyglutamic acid, which helps to improve the hemostatic effect and promote wound healing; at the same time, the amino-modified polyglutamic acid can also react with active groups such as hydroxyl and amino groups in type I collagen to improve the mechanical strength and stability of the hemostatic sponge;
[0040] 3. The specific porous starch microspheres used in this application have excellent water absorption performance and good biocompatibility, and can be used as a carrier of the hemostatic sponge to provide better moisture absorption and air permeability; at the same time, the addition of porous starch microspheres can also improve the flexibility and deformability of the hemostatic sponge, so that it can better adapt to the shape and changes of the wound;
[0041] 4. The preparation method of the absorbable collagen hemostatic sponge of the present application is simple to operate and suitable for large-scale production. At the same time, the prepared absorbable collagen hemostatic sponge has excellent comprehensive performance. DETAILED DESCRIPTION
[0042] The present application is further described in detail below with reference to the embodiments.
[0043] The raw material models of this application are as follows. Unless otherwise specified, the raw materials of this application are all commercially available:
[0044] Purified type I collagen: obtained by the preparation method of Preparation Example 1 in CN115227878A;
[0045] Polyglutamic acid: Hebei Ruqi Technology Co., Ltd., purity 99%;
[0046] Ammonia: Brand: Nanshi brand;
[0047] Ferric chloride: brand, Yuanfei, purity 98%;
[0048] Mannitol: Brand, Norlon, purity 99%;
[0049] Sodium sulfate: purity 99%.
[0050] Test items and methods:
[0051] According to "YY / T15112017 Collagen Sponge", the liquid absorbency and tensile resistance of the hemostatic sponge prepared in this application were tested; tensile resistance: the sponge was made into a strip with a width of 1 cm and a length of 10 cm, clamped at both ends with a clamp, and a tensile force was applied to it until it broke, and the tensile force value at the time of breaking was recorded.
[0052] Examples 1-5
[0053] The specific raw material weights of absorbable collagen hemostatic sponges of Examples 1-5 are shown in Table 1.
[0054] Table 1
[0055]
[0056] The average particle size of porous starch microspheres is 5 μm, and the specific surface area is 230 m 2 / g, amino-modified polyglutamic acid is prepared from polyglutamic acid, ammonia water and ferric chloride.
[0057] Example 1
[0058] A method for preparing an absorbable collagen hemostatic sponge comprises the following steps:
[0059] S1, dissolving amino-modified polyglutamic acid in 25 wt % acetic acid at a concentration of 0.03 mol / L to prepare solution 1;
[0060] S2, taking purified type I collagen and dissolving it in 25 wt % acetic acid at a concentration of 0.03 mol / L to prepare solution 2;
[0061] S3, dissolving the porous starch microspheres in the remaining acetic acid with a concentration of 0.03 mol / L to prepare solution 3;
[0062] S4, after mixing and stirring solution 1, solution 2 and solution 3, homogenizing them to obtain a slurry;
[0063] S5, pouring the slurry into a mold for freeze-drying to obtain the absorbable collagen hemostatic sponge;
[0064] Among them, in S1, the preparation method of amino-modified polyglutamic acid comprises the following steps: dissolving polyglutamic acid in water, adding ammonia water and ferric chloride, mixing and stirring for 1.5 hours at a temperature of 30°C, and then purifying to prepare amino-modified polyglutamic acid; wherein the weight ratio of polyglutamic acid, ammonia water and ferric chloride is 1:0.15:0.06, and the weight of water is twice the weight of polyglutamic acid.
[0065] Example 2
[0066] A method for preparing an absorbable collagen hemostatic sponge comprises the following steps:
[0067] S1, dissolving amino-modified polyglutamic acid in 32 wt % acetic acid at a concentration of 0.05 mol / L to prepare solution 1;
[0068] S2, taking purified type I collagen and dissolving it in 30 wt % acetic acid at a concentration of 0.05 mol / L to prepare solution 2;
[0069] S3, dissolving the porous starch microspheres in the remaining acetic acid with a concentration of 0.05 mol / L to prepare solution 3;
[0070] S4, mixing and stirring the solution 1, solution 2 and solution 3, and then homogenizing them to obtain a slurry;
[0071] S5, pouring the slurry into a mold for freeze-drying to obtain the absorbable collagen hemostatic sponge;
[0072] Among them, in S1, the preparation method of amino-modified polyglutamic acid comprises the following steps: dissolving polyglutamic acid in water, adding ammonia water and ferric chloride, mixing and stirring for 1.8 hours at a temperature of 35°C, and then purifying to prepare amino-modified polyglutamic acid; wherein the weight ratio of polyglutamic acid, ammonia water and ferric chloride is 1:0.2:0.07, and the weight of water is twice the weight of polyglutamic acid.
[0073] Example 3
[0074] A method for preparing an absorbable collagen hemostatic sponge comprises the following steps:
[0075] S1, dissolving amino-modified polyglutamic acid in 40 wt % acetic acid at a concentration of 0.06 mol / L to prepare solution 1;
[0076] S2, taking purified type I collagen and dissolving it in 40 wt % acetic acid at a concentration of 0.06 mol / L to prepare solution 2;
[0077] S3, dissolving the porous starch microspheres in the remaining acetic acid with a concentration of 0.06 mol / L to prepare solution 3;
[0078] S4, mixing and stirring the solution 1, solution 2 and solution 3, and then homogenizing them to obtain a slurry;
[0079] S5, pouring the slurry into a mold for freeze-drying to obtain the absorbable collagen hemostatic sponge;
[0080] Among them, in S1, the preparation method of amino-modified polyglutamic acid comprises the following steps: dissolving polyglutamic acid in water, adding ammonia water and ferric chloride, mixing and stirring for 2 hours at a temperature of 40°C, and then purifying to prepare amino-modified polyglutamic acid; wherein the weight ratio of polyglutamic acid, ammonia water and ferric chloride is 1:0.22:0.08, and the weight of water is twice the weight of polyglutamic acid.
[0081] The preparation method of Examples 4-5 is consistent with the preparation method of Example 2.
[0082] Comparative Example 1
[0083] Based on Example 2, except that an equal amount of polyglutamic acid was used to replace the amino-modified polyglutamic acid, the other components and preparation methods were the same as those in Example 2.
[0084] Comparative Example 2
[0085] Based on Example 2, except that amino-modified polyglutamic acid is not added, the other components and preparation methods are the same as those of Example 2.
[0086] Comparative Example 3
[0087] Based on Example 2, except that porous starch microspheres are not added, the other components and preparation methods are the same as those of Example 2.
[0088] The hemostatic sponges prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to performance tests, and the test results are shown in Table 2.
[0089] Table 2
[0090]
[0091]
[0092] It can be seen from Examples 1-3, Comparative Examples 1-3 and Table 2 that the hemostatic sponge prepared by the present application using specific raw materials has excellent hygroscopicity and flexibility, and can better adapt to the shape and changes of the wound;
[0093] It can be seen from Examples 4-5, 2 and Table 2 that the present application uses a better range of raw materials to prepare a hemostatic sponge with better comprehensive performance;
[0094] It can be seen from Comparative Examples 1-2, Example 2 and Table 2 that the present application uses a specific amino-modified polyglutamic acid to effectively improve the reactivity of polyglutamic acid and improve the water absorption of polyglutamic acid; at the same time, the amino-modified polyglutamic acid can also react with active groups such as hydroxyl groups and amino groups in type I collagen to improve the mechanical strength and stability of the hemostatic sponge;
[0095] It can be seen from Comparative Example 3, Example 2 and Table 2 that the specific porous starch microspheres used in the present application have excellent water absorption properties and good biocompatibility, and can be used as a carrier of the hemostatic sponge to provide better hygroscopicity and air permeability; at the same time, the addition of porous starch microspheres can also improve the flexibility and deformability of the hemostatic sponge, so that it can better adapt to the shape and changes of the wound.
[0096] Embodiment 6-7
[0097] Based on Example 4, except for the specific surface area of the porous starch microspheres, the other components and preparation methods are the same as those of Example 4.
[0098] Example 6
[0099] The specific surface area of porous starch microspheres is 300m 2 / g.
[0100] Example 7
[0101] The specific surface area of porous starch microspheres is 360 m 2 / g.
[0102] Embodiment 8-11
[0103] Based on Example 6, except for the average particle size of the porous starch microspheres, the other components and preparation methods are the same as those of Example 4.
[0104] Example 8
[0105] The average particle size of porous starch microspheres is 200 μm.
[0106] Example 9
[0107] The porous starch microspheres are composed of porous starch microspheres with an average particle size of 5 μm and porous starch microspheres with an average particle size of 82 μm in a weight ratio of 1:0.5.
[0108] Example 10
[0109] The porous starch microspheres are composed of porous starch microspheres with an average particle size of 45 μm and porous starch microspheres with an average particle size of 120 μm in a weight ratio of 1:0.6.
[0110] Embodiment 11
[0111] The porous starch microspheres are composed of porous starch microspheres with an average particle size of 80 μm and porous starch microspheres with an average particle size of 200 μm in a weight ratio of 1:0.8.
[0112] Examples 12-14
[0113] Based on Example 10, except that the porous starch microspheres are mannitol-modified porous starch microspheres, the other components and the preparation method are consistent with Example 10; wherein, the mannitol-modified porous starch microspheres are prepared from porous starch microspheres, mannitol and sodium sulfate, and the preparation method of the mannitol-modified porous starch microspheres is: dissolving the porous starch microspheres in water, adding mannitol and sodium sulfate, mixing and stirring at 120° C., reacting for 2 hours, purifying and drying, and preparing mannitol-modified porous starch microspheres, the weight of water is twice the weight of the porous starch microspheres.
[0114] Example 12
[0115] The weight ratio of porous starch microspheres, mannitol and sodium sulfate is 1:0.3:0.08.
[0116] Example 13
[0117] The weight ratio of porous starch microspheres, mannitol and sodium sulfate is 1:0.4:0.1.
[0118] Embodiment 14
[0119] The weight ratio of porous starch microspheres, mannitol and sodium sulfate is 1:0.5:0.12.
[0120] The hemostatic sponges prepared in Examples 6-12 were subjected to performance testing, and the test results are shown in Table 3.
[0121] Table 3
[0122] project Liquid absorption performance Tensile force / MPa Example 6 62.43 48.39 Example 7 62.32 48.36 Example 8 62.41 48.38 Example 9 62.58 48.52 Example 10 62.65 48.58 Embodiment 11 62.61 48.55 Example 12 62.83 48.85 Example 13 63.15 49.12 Embodiment 14 63.04 48.95
[0123] As can be seen from Examples 6-7, 4 and Table 3, the specific porous starch microspheres used in the present application have a high specific surface area and good water absorption performance, and as a carrier, provide better hygroscopicity and air permeability, and can also effectively improve the flexibility and deformability of the hemostatic sponge;
[0124] It can be seen from Examples 8-11, 6 and Table 3 that the present application uses porous starch microspheres with different particle sizes to form a hemostatic sponge with different pore sizes but uniform distribution. At the same time, a better filling effect is formed in the internal structure of the hemostatic sponge, so that the porous starch microspheres with different particle sizes can complement each other, thereby improving the overall flexibility and hygroscopicity of the hemostatic sponge.
[0125] It can be seen from Examples 12-14, 10 and Table 3 that the present application uses specific mannitol to modify the porous starch microspheres, so that the prepared hemostatic sponge has better hygroscopicity and flexibility, and can better adapt to the shape and changes of the wound; mannitol has good water absorption and flexibility. By combining mannitol with porous starch microspheres, the water absorption and flexibility of mannitol can be utilized to further improve the hygroscopicity and flexibility of the porous starch microspheres;
[0126] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, all equivalent changes made according to the principles of the present application should be included in the protection scope of the present application.
Claims
1. An absorbable collagen hemostatic sponge, characterized in that: The method comprises the following raw materials in parts by weight: 4.5-6.8 parts of amino-modified polyglutamic acid, 2.6-5.2 parts of purified type I collagen, 62-85 parts of acetic acid and 2.5-4 parts of porous starch microspheres; The amino-modified polyglutamic acid is prepared from raw materials including polyglutamic acid, ammonia water and ferric chloride in a weight ratio of 1:0.15-0.22:0.06-0.
08.
2. The absorbable collagen hemostatic sponge according to claim 1, characterized in that: The amino-modified polyglutamic acid is 5-5.6 parts, the purified type I collagen is 3.5-4.2 parts, the acetic acid is 70-78 parts and the porous starch microspheres are 3.2-3.5 parts.
3. The absorbable collagen hemostatic sponge according to claim 1, characterized in that: The specific surface area of the porous starch microspheres is 230-360 m 2 / g.
4. The absorbable collagen hemostatic sponge according to claim 1, characterized in that: The average particle size of the porous starch microspheres is 5-200 μm.
5. The absorbable collagen hemostatic sponge according to claim 4, characterized in that: The porous starch microspheres are composed of porous starch microspheres with an average particle size of 5-80 μm and porous starch microspheres with an average particle size of 80-200 μm in a weight ratio of 1:0.5-0.
8.
6. The absorbable collagen hemostatic sponge according to claim 1, characterized in that: The porous starch microspheres are mannitol-modified porous starch microspheres, which are prepared from raw materials including porous starch microspheres, mannitol and sodium sulfate in a weight ratio of 1:0.3-0.5:0.08-0.
12.
7. The absorbable collagen hemostatic sponge according to claim 1, characterized in that: The concentration of the acetic acid is 0.03-0.06 mol / L.
8. A method for preparing the absorbable collagen hemostatic sponge according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, dissolving amino-modified polyglutamic acid in 25-40wt% acetic acid to prepare solution 1; S2, dissolving purified type I collagen in 25-40 wt % acetic acid to prepare solution 2; S3, dissolving the porous starch microspheres in the remaining acetic acid to prepare solution 3; S4, mixing and stirring the solution 1, the solution 2 and the solution 3, and then homogenizing them to obtain a slurry; S5. Pour the slurry into a mold and perform freeze-drying treatment to obtain the absorbable collagen hemostatic sponge.
9. The method for preparing the absorbable collagen hemostatic sponge according to claim 8, characterized in that: In S1, the preparation method of amino-modified polyglutamic acid comprises the following steps: dissolving polyglutamic acid in water, adding ammonia water and ferric chloride, mixing and stirring, and then purifying to prepare amino-modified polyglutamic acid.
10. The method for preparing the absorbable collagen hemostatic sponge according to claim 9, characterized in that: The mixing and stirring temperature is 30-40° C., and the mixing and stirring time is 1.5-2 h.