A single phosphate rock powder binder-free granulation and drying process

Through the single phosphate powder binder-free granulation and drying process, the ball mill and pot granulator combined with three-stage drying technology were used to solve the problems of high bonding costs and insufficient ball strength in the existing technology, and realize the Efficient and low-cost phosphate powder pellet preparation improves the strength and utilization of the material ball.

CN117699753BActive Publication Date: 2024-12-06HENAN ZHENGZHOU MINING MACHINERY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311788621.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-12-06
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

The existing phosphate powder pellet process requires the addition of binder, which leads to high production costs and insufficient strength of finished balls, which cannot effectively solve the problems of phosphate powder accumulation and environmental pollution.

Method used

The single phosphate ore powder has no binder granulation and drying process is adopted, and the fine powder is formed through the ball milling mechanism. The high-efficiency granulator and the pot granulator are combined to make balls. Only a small amount of water is used, combined with three-stage drying technology to achieve high strength finished ball.

Benefits of technology

It realizes binder-free granulation, reduces production costs, improves the strength of the material ball, meets the transfer and furnace entry requirements of industrial production, and solves the problems of phosphate powder accumulation and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117699753B_ABST
    Figure CN117699753B_ABST
Patent Text Reader

Abstract

The invention discloses a single phosphate rock powder binder-free granulation and drying process method, which comprises the following steps: a. forming powder with suitable particle size by a ball mill powder selector; b. adopting a high-efficiency granulator to form balls as a starter, the particle size of the balls is Φ2-Φ5mm, and only water needs to be added in the process, the proportion is 10-13%, and the ball forming time is 5-8min; c. adding a starter of 10%-15% of the volume of a pot body, and by continuously replenishing powder and water, forming dense balls by layer coating during the continuous rotation of the pot-type granulator; d. the balls meeting the requirements enter the lower stage for drying, otherwise they return; e. firstly heating from room temperature to 105°C, keeping the temperature for 2 hours, then heating to 150°C, keeping the temperature for 2 hours, then heating to 900°C, keeping the temperature for 15 minutes, and finally cooling to room temperature to form finished balls. The invention does not need to use a binder and only needs a small amount of water to form high-strength material balls, which can fully meet the production and use of yellow phosphorus, thereby reducing production costs and solving the problem of difficult handling of large amounts of phosphate rock powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a pelletizing technology, in particular to a single phosphate rock powder binder-free granulation and drying process. Background Art

[0002] my country is a major country with important phosphate reserves and phosphorus chemical industry. Industrial phosphate is used to prepare phosphate products mostly by electric furnace method. The electric furnace method is to mix phosphate, silica and reducing agent and put them into the furnace for calcination, and finally produce high-quality phosphoric acid with less impurities. However, a large amount of powder ore will be produced in the process of phosphate mining. The powder rate of most phosphate ores exceeds 20%, and the highest can reach more than 50%. The powder ore cannot be directly used in the electric furnace, resulting in a large amount of tailings accumulation, and it will also cause environmental pollution problems.

[0003] How to solve this problem has been the exploration direction of domestic and foreign companies and experts for many years. At present, some companies add yellow phosphorus powder into organic fertilizers or use it as cement raw materials, but the amount added is not high enough to solve the current problem of large amounts of powder ore accumulation and its economic benefits are not high. Another way is to use yellow phosphorus powder in yellow phosphorus production after making balls. Domestic and foreign companies have long been exploring the process technology of phosphate rock powder pellets.

[0004] The existing phosphate rock pelletizing process usually adopts two processes, namely, the briquetting process and the ball making process. Among them, the briquetting process is to mix the phosphate rock powder, binder and water evenly and then put them into the roller briquetting machine to press the materials into Φ20-Φ30mm pellets at one time, and then dry and roast them to obtain finished balls. The ball making process is to mix the powder material and binder evenly and then add water in the disc granulator to make Φ20-Φ30mm pellets, and then dry and roast the obtained raw balls to make finished balls.

[0005] The two existing methods both require the addition of 4-8% binder during the ball making process, which increases the production cost by about 150-200 yuan per ton. Secondly, the raw material balls made by these two methods have a strength of only about 300N, and the strength is slightly reduced after drying and water loss. The strength is not enough. In industrial production, they are deformed, cracked, and crushed in large quantities during transportation into the furnace or even before entering the furnace, resulting in the inability of the phosphate rock powder to participate in the reaction and escape with the flue gas. The purpose of ball making cannot be achieved, and the normal operation of the electric furnace will also be affected. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a single phosphate rock powder binder-free granulation and drying process method with reasonable design, high strength and no binder.

[0007] The technical solution of the present invention is:

[0008] A single phosphate rock powder binder-free granulation and drying process method is characterized by comprising the following steps:

[0009] a. Grinding and powder selection: The powder ore produced by raw material phosphate mining is used as raw material, and the powder is made into 200-600 mesh powder by a ball mill powder selection mechanism;

[0010] b. High-efficiency granulation: Use high-efficiency granulator to make balls as the starter, the ball size is Φ2~Φ5mm, only water needs to be added during the process, the proportion is 10~13%, and the balling time is 5~8min;

[0011] c. Pot granulation: Add 10% to 15% of the pot volume of the starter, and continuously add powder and water. During the continuous rotation of the pot granulator, the pellets are coated layer by layer to form dense balls. The final ball size is Φ16 to Φ40 mm, the ball moisture is 9 to 15%, the ball making time is 2 to 3 hours, and the raw ball strength is 300 to 400N;

[0012] d. Ball screening: The balls produced in step c are screened, and the balls that meet the production requirements enter the next stage for drying;

[0013] e. Three-stage drying: The balls that meet the particle size requirements enter the drying system, first heated to 105°C at room temperature, kept at 105°C for 2 hours, then heated to 150°C, kept for 2 hours, then heated to 900°C, kept for 15 minutes, and finally cooled to room temperature to form balls. The balls have high strength, which can reach 3-4kN, which fully meets the requirement that the balls will not break during transportation before entering the calcining furnace.

[0014] Furthermore: in step e, the heating rate is 10°C / minute.

[0015] Further: in step d, the pellets with small particle size that do not meet the requirements are returned to the pot-type pelletizer and re-pelletized.

[0016] The beneficial effects of the present invention are:

[0017] 1. The present invention does not require the use of a binder and only requires a small amount of water to produce high-strength pellets, which fully meet the production and use of yellow phosphorus, thereby reducing production costs and solving the problem of difficult handling of large amounts of phosphate rock powder.

[0018] 2. The present invention adopts a high-efficiency granulation starter making and pot-type granulation combined with ball making, which only requires one raw material, phosphate rock powder, and does not require batching, pre-humidification, binder addition and stirring processes. It only needs to add an appropriate amount of water during granulation, saving the binder cost of the prior art. Usually, the binder addition amount is 4-8% (the conventional method of producing 1t requires an additive cost of about 140 yuan, and the adhesive is about 3,500 yuan per ton), which can save more than 30% of the production cost.

[0019] 3. The present invention adopts a three-stage drying technology. The ball-forming performance of phosphate rock powder itself is general, and it is very easy to burst during the drying and dehydration process. The present invention controls the heating rate and the insulation time to make the balls completely dehydrated without bursting, and then after being kept at 900°C for 15 minutes, the strength of 3-4kN can be achieved, which is much higher than the strength of the balls made by ordinary adhesives. The breakage rate is extremely low, so that the balls will not be broken and powdered during transportation before entering the furnace during industrial production, thereby improving the utilization rate after entering the furnace and reducing the flue gas treatment pressure.

[0020] 4. The control factors of seed pelleting by the high-efficiency granulator of the present invention are as follows: pellet size: Φ2-Φ5mm, pellet time: 5-8min, pellet moisture: 10-13%; good pelleting effect.

[0021] 5. The present invention has reasonable design, high strength, no use of adhesive, low production cost, and good economic benefits after promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a flow chart of a single phosphate rock powder binder-free granulation and drying process;

[0023] Figure 2 for Figure 1 Temperature curve of the middle three-stage drying. DETAILED DESCRIPTION

[0024] For example, see Figure 1 and Figure 2 , in the figure,

[0025] A single phosphate rock powder binder-free granulation and drying process method comprises the following steps:

[0026] 1. A single phosphate rock powder binder-free granulation and drying process, characterized in that it comprises the following steps:

[0027] a. Grinding and powder selection: The powder ore produced by raw material phosphate mining is used as raw material, and the powder is made into 200-600 mesh powder by a ball mill powder selection mechanism; the finer the particle size, the shorter the subsequent ball making time, and the better the sphericity and strength of the finished ball;

[0028] b. High-efficiency granulation: Use high-efficiency granulator to make balls as the starter, the ball size is Φ2~Φ5mm, only water needs to be added during the process, the proportion is 10~13%, and the balling time is 5~8min;

[0029] c. Pot granulation: Add 10% to 15% of the pot volume of the starter, and continuously add powder and water. During the continuous rotation of the pot granulator, the pellets are coated layer by layer to form dense balls. The final ball size is Φ16 to Φ40 mm, the ball moisture is 9 to 15%, the ball making time is 2 to 3 hours, and the raw ball strength is 300 to 400N;

[0030] d. Ball screening: The balls that meet the production requirements enter the lower stage for drying, and the balls that do not meet the requirements due to their small particle size return to the pot granulator for re-balling. The balls are added to the pot granulator together with the starter produced in step b;

[0031] e. Three-stage drying: The balls that meet the particle size requirements enter the drying system, first heated to 105°C at room temperature, kept at 105°C for 2 hours, then heated to 150°C, kept for 2 hours, then heated to 900°C, kept for 15 minutes, and finally cooled to room temperature to become finished balls. The balls have high strength, which can reach 3-4kN, which is much higher than the strength of balls made by ordinary adhesive pressing. The breakage rate is extremely low, which fully meets the requirement that the balls will not break during transportation before entering the furnace.

[0032] Preferred solution: In step e, the heating rate is 10°C / min. After drying, the product is transported to the next calcination stage, which can be calcined in an electric furnace. This is another process, which is not to be protected by the present invention and will not be described in detail.

[0033] Figure 2 In the figure, due to the length of the article, the time axis is not uniform, so the slope of the temperature curve is inconsistent. If the time axis is drawn in a one-to-one ratio, the slope of the heating curve is consistent.

[0034] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification made according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A single phosphate rock powder binder-free granulation and drying process, characterized in that : Includes the following steps: a. Grinding and powder selection: The powder ore produced by raw material phosphate mining is used as raw material, and the powder is made into 200-600 mesh powder by a ball mill powder selection mechanism; b. High-efficiency granulation: Use high-efficiency granulator to make balls as the starter, the ball size is Φ2~Φ5mm, only water needs to be added during the process, the proportion is 10~13%, and the balling time is 5~8min; c. Pot granulation: Add 10% to 15% of the pot volume of the starter, and continuously add powder and water. During the continuous rotation of the pot granulator, the pellets are coated layer by layer to form dense balls. The final ball size is Φ16 to Φ40 mm, the ball moisture is 9 to 15%, the ball making time is 2 to 3 hours, and the raw ball strength is 300 to 400N; d. Ball screening: The balls produced in step c are screened, and the balls that meet the production requirements enter the next stage for drying; e. Three-stage drying: The balls that meet the particle size requirements enter the drying system, first heated to 105°C at room temperature, kept at 105°C for 2 hours, then heated to 150°C, kept at 150°C for 2 hours, then heated to 900°C, kept at 15 minutes, and finally cooled to room temperature to form balls. The balls have high strength, reaching 3-4kN, which fully meets the requirement that the balls will not break during transportation before entering the calcining furnace; In step e, the heating rate is 10°C / min; In step d, the pellets with small particle sizes that do not meet the requirements are returned to the pot-type pelletizer and re-pelletized.

Citation Information

Patent Citations

  • Processing method for preparing phosphate rock powder into pellet yellow phosphorus charge

    CN102701164A

  • Composite pellet material used for kiln method phosphoric acid technology and molding method thereof

    CN104211028A

  • Improved method using rotary kiln for large scale production of phosphoric acid

    CN104211030A

  • Powdered rock phosphate pellet pressing, molding and roasting method

    CN104261362A

  • Efficient drying method for powdered rock phosphate pellets

    CN111646440A