Epoxy resin glue and copper clad laminate prepared therefrom

By reacting modified polyurethane prepolymer with epoxy resin, and combining it with long-chain flame retardants and modified silica, the problems of poor temperature resistance and flame retardancy of epoxy resin in copper clad laminates were solved, and copper clad laminates with high strength and good flame retardancy were prepared.

CN117700930BActive Publication Date: 2024-11-19NANTONG RODA ELECTRON
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311645671.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-04
Publication Date
2024-11-19
Estimated Expiration
2043-12-04

AI Technical Summary

Technical Problem

Epoxy resins used in copper-clad laminates suffer from poor temperature resistance, brittleness, and poor flame retardancy, which affect their performance.

Method used

By preparing a modified polyurethane prepolymer and reacting it with epoxy resin, combined with long-chain flame retardants and modified silica, the compatibility and cross-linking effect are improved, forming a more ordered structure and enhancing mechanical and flame retardant properties.

Benefits of technology

It improves the mechanical and flame-retardant properties of epoxy resin, avoids the problems of high brittleness and poor flame retardancy, and meets the high-temperature requirements of lead-free soldering.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of copper clad laminates, specifically to an epoxy resin glue and a copper clad laminate prepared therefrom. The present invention prepares a flame retardant by reacting phosphoric acid, polyethylene glycol 200 and N-phenylethylenediamine in a molar ratio of 1:1:1; hydroxy silicon dioxide is modified by isophorone diisocyanate at the same time, and the flame retardant is grafted onto the surface of the modified silicon dioxide to obtain flame retardant silicon dioxide; after flame retardant silicon dioxide and polyurethane prepolymer are mixed and modified, epoxy resin, acetone, butyl glycidyl ether, KH560, curing agent, 1-(β-cyanoethyl)-2-methylimidazole are blended to obtain epoxy resin glue with good flame retardancy and physical properties; after epoxy resin glue is applied to glass fiber cloth and semi-cured, copper foil is covered on the resin glue, hot pressed and cured to obtain a copper clad laminate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper clad laminates, in particular to an epoxy resin adhesive and a copper clad laminate prepared therefrom. Background Art

[0002] Copper clad laminate is used as the base material of printed circuit boards, which plays an important role in the performance and quality of printed circuit boards. In the preparation process of copper clad laminate, welding technology is often involved. Traditional welding technology uses cheap tin-lead alloy as solder. Although the quality of the product after welding is reliable, lead is a toxic heavy metal element that pollutes the ecological environment and endangers human health. For the concept of safety and environmental protection, lead-free welding technology has gradually become the mainstream. Compared with traditional welding technology, the temperature of lead-free welding is higher, which puts higher requirements on the heat resistance and thermal stability of printed circuit boards.

[0003] Epoxy resin is a high molecular polymer with excellent performance after curing, especially strong metal adhesion and strong chemical corrosion resistance. It has outstanding advantages in the application of copper clad laminates. However, epoxy resin also has disadvantages, and its temperature resistance is poor. Conventional modification methods mainly make up for the shortcomings of epoxy resin's insufficient temperature resistance by adding high-temperature resistant inorganic fillers. However, epoxy resin will phase separate from inorganic fillers, resulting in reduced mechanical properties and glass transition temperature of epoxy resin, and will also cause the cured epoxy resin to become brittle, affecting the quality of use. Therefore, it is very necessary to develop a high-temperature resistant epoxy resin glue and apply it to the preparation of copper clad laminates. Summary of the invention

[0004] The object of the present invention is to provide an epoxy resin adhesive and a copper clad laminate prepared therefrom, so as to solve the problems raised in the above-mentioned background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solution: an epoxy resin glue and a copper clad laminate prepared therefrom, comprising the following steps:

[0006] Step 1:

[0007] Mix polyethylene glycol 200 and phosphoric acid, react at 110-130° C. for 2-3 hours, cool to 40-50° C., add N-phenylethylenediamine, and stir to react for 1-2 hours to obtain a flame retardant;

[0008] Step 2:

[0009] S21: Weigh hydroxy silica and isophorone diisocyanate, add them to N,N-dimethylformamide, add dibutyltin dilaurate as a catalyst dropwise under a nitrogen environment, raise the temperature to 70-90° C., stir for 24-36 hours to obtain a suspension; centrifuge the suspension, filter out the filtrate, and wash the filter residue with ethanol to obtain modified silica;

[0010] S22: Mix and disperse the flame retardant and modified silica in N,N-dimethylformamide, dropwise add dibutyltin dilaurate as a catalyst under a nitrogen environment, raise the temperature to 70-90° C. and react for 2-3 hours to obtain flame retardant silica;

[0011] Step 3:

[0012] After dehydrating and cooling the raw materials at 110-120° C., adding isophorone diisocyanate to polyethylene glycol 2000, reacting at 80-90° C. for 2-3 hours, continuing to add dimethylolpropionic acid, 1,4-butanediol, and flame-retardant silica, dropping a catalyst dibutyltin dilaurate into the mixed system, raising the temperature to 80-90° C. for 2-3 hours, and obtaining a modified polyurethane prepolymer;

[0013] Step 4:

[0014] The epoxy resin and modified polyurethane prepolymer are mixed to obtain a mixed adhesive solution; the mixed adhesive solution, acetone, butyl glycidyl ether and KH560 are mixed, stirred at a stirring rate of 800 to 1000 rpm for 10 to 30 minutes, and a curing agent and 1-(β-cyanoethyl)-2-methylimidazole are added to obtain an epoxy resin adhesive solution; the epoxy resin adhesive solution is coated on a glass fiber cloth, and after semi-curing, a copper foil is covered on the resin adhesive solution, and hot pressing and curing are performed to obtain a copper clad laminate.

[0015] Furthermore, in step 1, the molar ratio of phosphoric acid, polyethylene glycol 200 and N-phenylethylenediamine is 1:1:1.

[0016] Furthermore, in step S21, the weight ratio of hydroxy silica, isophorone diisocyanate, and N,N-dimethylformamide is (3-5):(10-15):100.

[0017] Furthermore, in step S22, by weight, 10 to 15 parts of flame retardant and 3 to 5 parts of modified silica are used.

[0018] Furthermore, in step 3, the content of each component in the modified polyurethane prepolymer, by weight, is 100 to 120 parts of polyethylene glycol 2000, 70 to 80 parts of isophorone diisocyanate, 0.8 to 1.1 parts of dihydroxymethylpropionic acid, 0.2 to 0.25 parts of 1,4-butanediol, and 15 to 20 parts of flame retardant silica.

[0019] Furthermore, in step 4, the mixed glue contains 85-90% epoxy resin and 10-15% modified polyurethane prepolymer.

[0020] Furthermore, in step 4, the contents of the components in the epoxy resin adhesive are, by weight, 120 to 150 parts of mixed adhesive, 45 to 50 parts of modified polyurethane prepolymer, 25 to 34 parts of acetone, 15 to 18 parts of butyl glycidyl ether, 8 to 12 parts of KH560, 25 to 30 parts of curing agent, and 1 to 2 parts of 1-(β-cyanoethyl)-2-methylimidazole.

[0021] Furthermore, in step 4, the curing agent is any one of ethylenediamine, hexamethylenediamine, diethylenetriamine, maleic anhydride, tetraethylenepentamine, phthalic anhydride, phenolic resin, and dicyandiamide.

[0022] Furthermore, in step 4, the semi-curing temperature is 100-120° C. and the time is 5-10 minutes.

[0023] Furthermore, in step 4, the hot pressing temperature is 180-200° C. and the pressure is 2-2.5 MPa.

[0024] Compared with the prior art, the beneficial effect achieved by the present invention is that the present invention applies epoxy resin glue to prepare copper clad laminates. In order to solve the problems of high brittleness and poor flame retardant performance of epoxy resin after curing, the present invention uses polyethylene glycol 2000 to prepare modified polyurethane prepolymer, and modifies epoxy resin, and the isocyanate-terminated polyurethane prepolymer reacts with the hydroxyl group in the epoxy resin to make the compatibility of the two better. The introduction of polyurethane prepolymer can improve the mechanical properties of epoxy resin, including tensile strength and toughness, and effectively avoid the problem of high brittleness of epoxy resin after curing.

[0025] In order to improve the flame retardant properties of epoxy resin, the present invention prepares a long-chain flame retardant, controls the molar ratio of phosphoric acid, polyethylene glycol 200 and N-phenylethylenediamine to 1:1:1, so that the hydroxyl group of polyethylene glycol 200 is not completely reacted; uses isophorone diisocyanate to modify hydroxyl silica, and then reacts the hydroxyl group on the flame retardant with the isocyanate group on the silica to obtain flame retardant silica. The flame retardant prepared with polyethylene glycol 200 as a raw material, on the one hand, makes the flame retardant and the polyurethane prepolymer have a similar structure, and improves the dispersion performance of flame retardant silica; on the other hand, the introduction of long-chain molecules forms a more ordered structure in the epoxy resin, which enhances the interaction between the two. In addition, low molecular weight polyethylene glycol 200 can also avoid the excessive steric hindrance effect of the flame retardant molecule, affecting the reaction of the isocyanate group on the surface of silica with the hydroxyl group in the epoxy resin, thereby improving the cross-linking effect of silica and epoxy resin. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Materials used in the present invention and their sources: polyethylene glycol 200 and polyethylene glycol 2000 are from Guoli Chemical; hydroxy silicon dioxide is from Anbiqi Biotechnology, model DNG-B001; epoxy resin E51 is from Linyuan Fine Chemical; and the curing agent is dicyandiamide, which is from Aladdin.

[0028] Embodiment 1: An epoxy resin glue and a copper-clad laminate prepared therefrom, comprising the following steps:

[0029] Step 1:

[0030] 1 mol of polyethylene glycol 200 and 1 mol of phosphoric acid were mixed, reacted at 110°C for 2 hours, cooled to 40°C, 1 mol of N-phenylethylenediamine was added, and stirred for 1 hour to obtain a flame retardant;

[0031] Step 2:

[0032] S21: 5 g of silica and 15 g of isophorone diisocyanate were weighed and added to 100 g of N,N-dimethylformamide, 0.03 g of catalyst dibutyltin dilaurate was added dropwise under nitrogen atmosphere, the temperature was raised to 80° C., and stirring was continued for 24 h to obtain a suspension; the suspension was centrifuged, the filtrate was filtered out, and the filter residue was washed with ethanol to obtain modified silica;

[0033] S22: 10 g of flame retardant and 3 g of modified silica were mixed and dispersed in N,N-dimethylformamide, 0.03 g of catalyst dibutyltin dilaurate was added dropwise under nitrogen environment, and the temperature was raised to 70° C. for reaction for 2 h to obtain flame retardant silica;

[0034] Step 3:

[0035] After dehydrating and cooling the raw materials at 110° C., 75 g of isophorone diisocyanate was added to 100 g of polyethylene glycol 2000, and the mixture was reacted at 80° C. for 2 h in a nitrogen environment. 1.1 g of dimethylolpropionic acid, 0.25 g of 1,4-butanediol, and 20 g of flame-retardant silica were added, and a catalyst of dibutyltin dilaurate (accounting for 0.1% of the total mass of the mixture) was added dropwise to the mixture, and the mixture was heated to 80° C. for 2 h to obtain a modified polyurethane prepolymer;

[0036] Step 4:

[0037] 90% of epoxy resin E51 and 10% of modified polyurethane prepolymer are mixed by weight to obtain a mixed glue solution, 25g of acetone, 15g of butyl glycidyl ether and 12g of KH560 are added to 120g of the mixed glue solution, and the mixture is stirred at a stirring rate of 800rpm for 10min, and 30g of a curing agent and 1g of 1-(β-cyanoethyl)-2-methylimidazole are added to obtain an epoxy resin glue solution; the epoxy resin glue solution is coated on a glass fiber cloth, semi-cured at 100°C for 5min, and then a copper foil is covered on the resin glue solution, and hot pressed and cured at 180°C and 2MPa to obtain a copper clad laminate.

[0038] Embodiment 2: An epoxy resin glue and a copper-clad laminate prepared therefrom, comprising the following steps:

[0039] Step 1:

[0040] 1 mol of polyethylene glycol 200 and 1 mol of phosphoric acid were mixed, reacted at 115°C for 2.5 hours, cooled to 45°C, 1 mol of N-phenylethylenediamine was added, and stirred for 1.5 hours to obtain a flame retardant;

[0041] Step 2:

[0042] S21: 5 g of silica and 15 g of isophorone diisocyanate were weighed and added to 100 g of N,N-dimethylformamide, 0.03 g of dibutyltin dilaurate as a catalyst was added dropwise under a nitrogen environment, the temperature was raised to 85° C., and stirring was continued for 30 h to obtain a suspension; the suspension was centrifuged, the filtrate was filtered out, and the filter residue was washed with ethanol to obtain modified silica;

[0043] S22: 10 g of flame retardant and 3 g of modified silica were mixed and dispersed in N,N-dimethylformamide, 0.03 g of catalyst dibutyltin dilaurate was added dropwise under nitrogen environment, and the temperature was raised to 80° C. for reaction for 2.5 h to obtain flame retardant silica;

[0044] Step 3:

[0045] After dehydrating and cooling the raw materials at 115° C., 75 g of isophorone diisocyanate was added to 100 g of polyethylene glycol 2000, and the mixture was reacted at 85° C. for 2.5 h in a nitrogen environment. 1.1 g of dimethylolpropionic acid, 0.25 g of 1,4-butanediol, and 20 g of flame-retardant silica were added, and a catalyst of dibutyltin dilaurate (accounting for 0.1% of the total mass of the mixture) was added dropwise to the mixture, and the mixture was heated to 85° C. and reacted for 2.5 h to obtain a modified polyurethane prepolymer;

[0046] Step 4:

[0047] 90% of epoxy resin E51 and 10% of modified polyurethane prepolymer are mixed by weight to obtain a mixed glue solution, 25g of acetone, 15g of butyl glycidyl ether and 12g of KH560 are added to 120g of the mixed glue solution, and the mixture is stirred at a stirring rate of 900rpm for 15min, and 30g of a curing agent and 1g of 1-(β-cyanoethyl)-2-methylimidazole are added to obtain an epoxy resin glue solution; the epoxy resin glue solution is coated on a glass fiber cloth, semi-cured at 110°C for 8min, and then a copper foil is covered on the resin glue solution, and hot pressed and cured at 190°C and 2.3MPa to obtain a copper clad laminate.

[0048] Embodiment 3: An epoxy resin glue and a copper-clad laminate prepared therefrom, comprising the following steps:

[0049] Step 1:

[0050] 1 mol of polyethylene glycol 200 and 1 mol of phosphoric acid were mixed, reacted at 130°C for 3 hours, cooled to 50°C, 1 mol of N-phenylethylenediamine was added, and stirred for reaction for 2 hours to obtain a flame retardant;

[0051] Step 2:

[0052] S21: 5 g of silica and 15 g of isophorone diisocyanate were weighed and added to 100 g of N,N-dimethylformamide, 0.03 g of dibutyltin dilaurate as a catalyst was added dropwise under a nitrogen environment, the temperature was raised to 90° C., and stirring was continued for 36 hours to obtain a suspension; the suspension was centrifuged, the filtrate was filtered out, and the filter residue was washed with ethanol to obtain modified silica;

[0053] S22: 10 g of flame retardant and 3 g of modified silica were mixed and dispersed in N,N-dimethylformamide, 0.03 g of catalyst dibutyltin dilaurate was added dropwise under nitrogen environment, and the temperature was raised to 90° C. for reaction for 3 h to obtain flame retardant silica;

[0054] Step 3:

[0055] After dehydrating and cooling the raw materials at 120° C., 75 g of isophorone diisocyanate was added to 100 g of polyethylene glycol 2000, and the mixture was reacted for 3 h under a nitrogen environment at 90° C., 1.1 g of dimethylolpropionic acid, 0.25 g of 1,4-butanediol, and 20 g of flame-retardant silica were added, and a catalyst of dibutyltin dilaurate (accounting for 0.1% of the total mass of the mixture) was added dropwise to the mixture, and the mixture was heated to 90° C. and reacted for 3 h to obtain a modified polyurethane prepolymer;

[0056] Step 4:

[0057] 90% of epoxy resin E51 and 10% of modified polyurethane prepolymer are mixed by weight to obtain a mixed glue solution, 25g of acetone, 15g of butyl glycidyl ether and 12g of KH560 are added to 120g of the mixed glue solution, and the mixture is stirred at a stirring rate of 1000rpm for 30min, and 30g of a curing agent and 1g of 1-(β-cyanoethyl)-2-methylimidazole are added to obtain an epoxy resin glue solution; the epoxy resin glue solution is coated on a glass fiber cloth, semi-cured at 120°C for 10min, and then a copper foil is covered on the resin glue solution, and hot pressed and cured at 200°C and 2.5MPa to obtain a copper clad laminate.

[0058] Embodiment 4: An epoxy resin glue and a copper-clad laminate prepared therefrom, comprising the following steps:

[0059] Step 1:

[0060] 1 mol of polyethylene glycol 200 and 1 mol of phosphoric acid were mixed, reacted at 130°C for 3 hours, cooled to 50°C, 1 mol of N-phenylethylenediamine was added, and stirred for reaction for 2 hours to obtain a flame retardant;

[0061] Step 2:

[0062] S21: 5 g of silica and 15 g of isophorone diisocyanate were weighed and added to 100 g of N,N-dimethylformamide, 0.03 g of dibutyltin dilaurate as a catalyst was added dropwise under a nitrogen environment, the temperature was raised to 80° C., and stirring was continued for 36 h to obtain a suspension; the suspension was centrifuged, the filtrate was filtered out, and the filter residue was washed with ethanol to obtain modified silica;

[0063] S22: 10 g of flame retardant and 3 g of modified silica were mixed and dispersed in N,N-dimethylformamide, 0.03 g of catalyst dibutyltin dilaurate was added dropwise under nitrogen environment, and the temperature was raised to 70° C. for reaction for 3 h to obtain flame retardant silica;

[0064] Step 3:

[0065] After dehydrating and cooling the raw materials at 120° C., 75 g of isophorone diisocyanate was added to 100 g of polyethylene glycol 2000, and the mixture was reacted for 3 h under a nitrogen environment at 90° C., 1.1 g of dimethylolpropionic acid, 0.25 g of 1,4-butanediol, and 20 g of flame-retardant silica were added, and a catalyst of dibutyltin dilaurate (accounting for 0.1% of the total mass of the mixture) was added dropwise to the mixture, and the mixture was heated to 90° C. and reacted for 3 h to obtain a modified polyurethane prepolymer;

[0066] Step 4:

[0067] In percentage by weight, 88% epoxy resin E51 and 12% modified polyurethane prepolymer are mixed to obtain a mixed glue solution, 25g acetone, 15g butyl glycidyl ether and 12g KH560 are added to 120g of the mixed glue solution, and the mixture is stirred at a stirring rate of 850rpm for 20min, and 30g curing agent and 1g 1-(β-cyanoethyl)-2-methylimidazole are added to obtain epoxy resin glue solution; the epoxy resin glue solution is coated on a glass fiber cloth, semi-cured at 100°C for 10min, and then a copper foil is covered on the resin glue solution, and hot pressed and cured at 185°C and 2MPa to obtain a copper clad laminate.

[0068] Embodiment 5: An epoxy resin glue and a copper-clad laminate prepared therefrom, comprising the following steps:

[0069] Step 1:

[0070] 1 mol of polyethylene glycol 200 and 1 mol of phosphoric acid were mixed, reacted at 125°C for 2.5 hours, cooled to 45°C, 1 mol of N-phenylethylenediamine was added, and stirred for reaction for 1.5 hours to obtain a flame retardant;

[0071] Step 2:

[0072] S21: 5 g of silica and 15 g of isophorone diisocyanate were weighed and added to 100 g of N,N-dimethylformamide, 0.03 g of dibutyltin dilaurate as a catalyst was added dropwise under a nitrogen environment, the temperature was raised to 80° C., and stirring was continued for 30 h to obtain a suspension; the suspension was centrifuged, the filtrate was filtered out, and the filter residue was washed with ethanol to obtain modified silica;

[0073] S22: 10 g of flame retardant and 3 g of modified silica were mixed and dispersed in N,N-dimethylformamide, 0.03 g of catalyst dibutyltin dilaurate was added dropwise under nitrogen environment, and the temperature was raised to 70° C. for reaction for 2.5 h to obtain flame retardant silica;

[0074] Step 3:

[0075] After dehydrating and cooling the raw materials at 120° C., 75 g of isophorone diisocyanate was added to 100 g of polyethylene glycol 2000, and the mixture was reacted at 85° C. for 2.5 h in a nitrogen environment. 1.1 g of dimethylolpropionic acid, 0.25 g of 1,4-butanediol, and 20 g of flame-retardant silica were added, and a catalyst of dibutyltin dilaurate (accounting for 0.1% of the total mass of the mixture) was added dropwise to the mixture, and the mixture was heated to 85° C. for 3 h to obtain a modified polyurethane prepolymer;

[0076] Step 4:

[0077] In percentage by weight, 87% epoxy resin E51 and 13% modified polyurethane prepolymer are mixed to obtain a mixed glue solution, 25g acetone, 15g butyl glycidyl ether and 12g KH560 are added to 120g of the mixed glue solution, and the mixture is stirred at a stirring rate of 950rpm for 25min, and 30g curing agent and 1g 1-(β-cyanoethyl)-2-methylimidazole are added to obtain epoxy resin glue solution; the epoxy resin glue solution is coated on a glass fiber cloth, semi-cured at 120°C for 5min, and then a copper foil is covered on the resin glue solution, and hot pressed and cured at 200°C and 2MPa to obtain a copper clad laminate.

[0078] Embodiment 6: An epoxy resin glue and a copper-clad laminate prepared therefrom, comprising the following steps:

[0079] Step 1:

[0080] 1 mol of polyethylene glycol 200 and 1 mol of phosphoric acid were mixed, reacted at 110°C for 2.5 hours, cooled to 45°C, 1 mol of N-phenylethylenediamine was added, and stirred for 1 hour to obtain a flame retardant;

[0081] Step 2:

[0082] S21: 5 g of silica and 15 g of isophorone diisocyanate were weighed and added to 100 g of N,N-dimethylformamide, 0.03 g of dibutyltin dilaurate as a catalyst was added dropwise under a nitrogen environment, the temperature was raised to 80° C., and stirring was continued for 36 h to obtain a suspension; the suspension was centrifuged, the filtrate was filtered out, and the filter residue was washed with ethanol to obtain modified silica;

[0083] S22: 10 g of flame retardant and 3 g of modified silica were mixed and dispersed in N,N-dimethylformamide, 0.03 g of catalyst dibutyltin dilaurate was added dropwise under nitrogen environment, and the temperature was raised to 70° C. for reaction for 3 h to obtain flame retardant silica;

[0084] Step 3:

[0085] After dehydrating and cooling the raw materials at 120° C., 75 g of isophorone diisocyanate was added to 100 g of polyethylene glycol 2000, and the mixture was reacted for 3 h in a nitrogen environment at 80° C., 1.1 g of dimethylolpropionic acid, 0.25 g of 1,4-butanediol, and 20 g of flame-retardant silica were added, and a catalyst of dibutyltin dilaurate (accounting for 0.1% of the total mass of the mixture) was added dropwise to the mixture, and the mixture was heated to 90° C. and reacted for 2 h to obtain a modified polyurethane prepolymer;

[0086] Step 4:

[0087] 85% epoxy resin E51 and 15% modified polyurethane prepolymer were mixed by weight to obtain a mixed glue solution, 25g acetone, 15g butyl glycidyl ether and 12g KH560 were added to 120g of the mixed glue solution, and the mixture was stirred at a stirring rate of 1000rpm for 10min, and 30g curing agent and 1g 1-(β-cyanoethyl)-2-methylimidazole were added to obtain epoxy resin glue solution; the epoxy resin glue solution was coated on a glass fiber cloth, semi-cured at 120°C for 10min, and then a copper foil was covered on the resin glue solution, and hot pressed and cured at 200°C and 2.5MPa to obtain a copper clad laminate.

[0088] Comparative Example 1: No modified polyurethane prepolymer is used for mixing with the epoxy resin, and other parameters are the same as those in Example 1.

[0089] Add 25g of acetone, 15g of butyl glycidyl ether and 12g of KH560 to 120g of the mixed adhesive, stir at a stirring rate of 800rpm for 10min, add 30g of curing agent and 1g of 1-(β-cyanoethyl)-2-methylimidazole to obtain epoxy resin adhesive; apply the epoxy resin adhesive on glass fiber cloth, semi-cured at 100°C for 5min, cover copper foil on the resin adhesive, hot press and cure at 180°C and 2MPa to obtain a copper clad laminate.

[0090] Comparative Example 2: The flame retardant silica in step 3 was replaced by conventional silica, and the other parameters were the same as those in Example 2.

[0091] Step 1:

[0092] After dehydrating and cooling the raw materials at 115° C., 75 g of isophorone diisocyanate was added to 100 g of polyethylene glycol 2000, and the mixture was reacted at 85° C. for 2.5 h in a nitrogen environment. 1.1 g of dimethylolpropionic acid, 0.25 g of 1,4-butanediol, and 20 g of silicon dioxide were added, and a catalyst of dibutyltin dilaurate (accounting for 0.1% of the total mass of the mixture) was added dropwise to the mixture, and the mixture was heated to 85° C. and reacted for 2.5 h to obtain a modified polyurethane prepolymer;

[0093] Step 2:

[0094] 90% of epoxy resin E51 and 10% of modified polyurethane prepolymer are mixed by weight to obtain a mixed glue solution, 25g of acetone, 15g of butyl glycidyl ether and 12g of KH560 are added to 120g of the mixed glue solution, and the mixture is stirred at a stirring rate of 900rpm for 15min, and 30g of a curing agent and 1g of 1-(β-cyanoethyl)-2-methylimidazole are added to obtain an epoxy resin glue solution; the epoxy resin glue solution is coated on a glass fiber cloth, semi-cured at 110°C for 8min, and then a copper foil is covered on the resin glue solution, and hot pressed and cured at 190°C and 2.3MPa to obtain a copper clad laminate.

[0095] Comparative Example 3: The amount of phosphoric acid in step 1 was increased, and the other parameters were the same as those in Example 3.

[0096] Step 1:

[0097] 1 mol of polyethylene glycol 200 and 3 mol of phosphoric acid were mixed, reacted at 130°C for 3 h, cooled to 50°C, 1 mol of N-phenylethylenediamine was added, and stirred for 2 h to obtain a flame retardant;

[0098] Step 2:

[0099] S21: 5 g of silica and 15 g of isophorone diisocyanate were weighed and added to 100 g of N,N-dimethylformamide, 0.03 g of dibutyltin dilaurate as a catalyst was added dropwise under a nitrogen environment, the temperature was raised to 90° C., and stirring was continued for 36 h to obtain a suspension; the suspension was centrifuged, the filtrate was filtered out, and the filter residue was washed with ethanol to obtain modified silica;

[0100] S22: 10 g of flame retardant and 3 g of modified silica were mixed and dispersed in N,N-dimethylformamide, 0.03 g of catalyst dibutyltin dilaurate was added dropwise under nitrogen environment, and the temperature was raised to 90° C. for reaction for 3 h to obtain flame retardant silica;

[0101] Step 3:

[0102] After dehydrating and cooling the raw materials at 120° C., 75 g of isophorone diisocyanate was added to 100 g of polyethylene glycol 2000, and the mixture was reacted for 3 h under a nitrogen environment at 90° C., 1.1 g of dimethylolpropionic acid, 0.25 g of 1,4-butanediol, and 20 g of flame-retardant silica were added, and a catalyst of dibutyltin dilaurate (accounting for 0.1% of the total mass of the mixture) was added dropwise to the mixture, and the mixture was heated to 90° C. and reacted for 3 h to obtain a modified polyurethane prepolymer;

[0103] Step 4:

[0104] 90% of epoxy resin E51 and 10% of modified polyurethane prepolymer are mixed by weight to obtain a mixed glue solution, 25g of acetone, 15g of butyl glycidyl ether and 12g of KH560 are added to 120g of the mixed glue solution, and the mixture is stirred at a stirring rate of 1000rpm for 30min, and 30g of a curing agent and 1g of 1-(β-cyanoethyl)-2-methylimidazole are added to obtain an epoxy resin glue solution; the epoxy resin glue solution is coated on a glass fiber cloth, semi-cured at 120°C for 10min, and then a copper foil is covered on the resin glue solution, and hot pressed and cured at 200°C and 2.5MPa to obtain a copper clad laminate.

[0105] Experiment: The epoxy resin adhesives prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were tested, and the epoxy resin adhesives were cured into sample strips of 10 cm×3 cm×0.1 cm. The results are shown in the following table.

[0106] The tensile strength and elongation at break test methods were both tested using a HY-5080 universal tensile testing machine at a test speed of 50 mm / min;

[0107] Flame retardancy test: The epoxy resin glue was cured to form a sample strip of 10cm×1cm×0.5cm, which was burned with an open flame for 30s and then removed to observe whether it was burning.

[0108] project Tensile strength / MPa Elongation at break / % Flame retardant properties Example 1 34 25.4 non-flammable Example 2 34 25.4 non-flammable Example 3 34 25.4 non-flammable Example 4 35 26.7 non-flammable Example 5 37 27.4 non-flammable Example 6 38 28.1 non-flammable Comparative Example 1 31 21.6 combustion Comparative Example 2 32 24.3 combustion Comparative Example 3 34 25.1 combustion

[0109] Conclusion: The data of Examples 1 to 6 show that the epoxy resin glue prepared by the present invention has good flame retardant properties and physical strength, and can be used to prepare copper clad laminates. The data of Example 1 and Comparative Example 1 show that after adding the modified polyurethane prepolymer, the epoxy resin has good flame retardant properties, tensile strength and elongation at break; the data of Example 2 and Comparative Example 2 show that flame retardant silica can impart flame retardant properties and improve the physical properties of epoxy resin materials; the data of Example 3 and Comparative Example 3 show that when preparing a flame retardant, after increasing the amount of phosphoric acid, the hydroxyl groups on polyethylene glycol 200 are completely reacted, and silica cannot be grafted with the flame retardant, so the flame retardant effect is not good.

[0110] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an epoxy resin glue, characterized in that: The following steps are involved: Step 1: After dehydrating and cooling the raw materials at 110-120° C., adding isophorone diisocyanate to polyethylene glycol 2000, reacting for 2-3 hours at 80-90° C. in a nitrogen environment, continuing to add dimethylolpropionic acid, 1,4-butanediol, and flame-retardant silica, dropping a catalyst dibutyltin dilaurate into the mixed system, raising the temperature to 80-90° C. to react for 2-3 hours, and obtaining a modified polyurethane prepolymer; The method for preparing flame retardant silicon dioxide comprises the following steps: S1: Mix polyethylene glycol 200 and phosphoric acid, react at 110-130° C. for 2-3 hours, cool to 40-50° C., add N-phenylethylenediamine, and stir to react for 1-2 hours to obtain a flame retardant; wherein the molar ratio of phosphoric acid, polyethylene glycol 200 and N-phenylethylenediamine is 1:1:1; S2: Weigh hydroxy silica and isophorone diisocyanate, add them to N,N-dimethylformamide, add dibutyltin dilaurate as a catalyst dropwise under nitrogen, raise the temperature to 70-90°C, stir for 24-36 hours to obtain a suspension; centrifuge the suspension, filter out the filtrate, wash the filter residue with ethanol to obtain modified silica; wherein the weight ratio of hydroxy silica, isophorone diisocyanate and N,N-dimethylformamide is (3-5):(10-15):100; S3: By weight, 10 to 15 parts of flame retardant and 3 to 5 parts of modified silica are mixed and dispersed in N,N-dimethylformamide, and a catalyst dibutyltin dilaurate is added dropwise under a nitrogen environment, and the temperature is raised to 70 to 90° C. and reacted for 2 to 3 hours to obtain flame retardant silica; Step 2: The epoxy resin and the modified polyurethane prepolymer are mixed to obtain a mixed glue solution; the mixed glue solution, acetone, butyl glycidyl ether and KH560 are mixed, stirred at a stirring rate of 800 to 1000 rpm for 10 to 30 minutes, and a curing agent and 1-(β-cyanoethyl)-2-methylimidazole are added to obtain an epoxy resin glue solution.

2. The method for preparing an epoxy resin glue according to claim 1, characterized in that: In step 1, the content of each component in the modified polyurethane prepolymer, by weight, is 100 to 120 parts of polyethylene glycol 2000, 70 to 80 parts of isophorone diisocyanate, 0.8 to 1.1 parts of dihydroxymethylpropionic acid, 0.2 to 0.25 parts of 1,4-butanediol, and 15 to 20 parts of flame retardant silica.

3. The method for preparing an epoxy resin glue according to claim 1, characterized in that: In step 2, the contents of the components in the epoxy resin adhesive are, by weight, 120 to 150 parts of mixed adhesive, 25 to 34 parts of acetone, 15 to 18 parts of butyl glycidyl ether, 8 to 12 parts of KH560, 25 to 30 parts of curing agent, and 1 to 2 parts of 1-(β-cyanoethyl)-2-methylimidazole.

4. The method for preparing an epoxy resin glue according to claim 1, characterized in that: In step 2, the curing agent is any one of ethylenediamine, hexamethylenediamine, diethylenetriamine, maleic anhydride, tetraethylenepentamine, phthalic anhydride, phenolic resin, and dicyandiamide.

5. An epoxy resin adhesive prepared by the preparation method according to any one of claims 1 to 4.

6. A copper clad laminate prepared by the epoxy resin adhesive as claimed in claim 5, characterized in that: The epoxy resin adhesive is coated on the glass fiber cloth, semi-cured at 100-120°C for 5-10 minutes, and then the copper foil is covered on the resin adhesive. The copper foil is hot-pressed and cured at 180-200°C and 2-2.5MPa to obtain a copper clad laminate.