Preparation method and application of cobalt and strontium selective adsorption reagent material

Through the combined use of silicate materials and reagents, highly selective cobalt and strontium selective adsorption reagent materials are prepared, and the problem of low strontium/calcium selectivity in the existing technology is solved by utilizing ion exchange and co-precipitation. It significantly improves the treatment efficiency of 60Co and 90Sr in radioactive wastewater, enhances the adsorption efficiency and reduces the amount of waste resin produced.

CN117732423BActive Publication Date: 2024-10-11NAVAL UNIV OF ENG PLA
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202311840329.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2024-10-11
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

When existing ion exchange resins treat radioactive wastewater with high salt content, their strontium/calcium selectivity is low, resulting in inefficient treatment of strontium and cobalt, reducing utilization efficiency and increasing the amount of waste resin produced.

Method used

Using silicate materials and reagents in combination, through ion exchange and co-precipitation on the adsorption reagent materials, highly selective cobalt and strontium selective adsorption reagent materials are prepared, using amorphous barium silicate and SO42 -, PO43-, CO32-, etc. work together to achieve the selective removal of 60Co and 90Sr.

Benefits of technology

The material's selectivity for 60Co and 90Sr in high-salt radioactive wastewater is significantly improved, the adsorption efficiency is improved, the interference with Ca2+ and Mg2+ is reduced, and the utilization efficiency of ion exchange resin is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004638611410000041
    Figure BDA0004638611410000041
  • Figure BDA0004638611410000051
    Figure BDA0004638611410000051
  • Figure BDA0004638611410000052
    Figure BDA0004638611410000052
Patent Text Reader

Abstract

The present invention relates to a preparation method and application of a cobalt and strontium selective adsorption reagent material, the steps of which include fully mixing silicon dioxide and sodium hydroxide in deionized water to obtain silica sol, then mixing with a certain amount of barium chloride solution, stirring, settling, skimming off the supernatant and filtering, and drying the obtained product to obtain an adsorption reagent material. The adsorption reagent material is mixed with SO4 in radioactive wastewater. 2‑ PO4 3‑ 、CO3 2‑ Through the combined action of ion exchange and co-precipitation on the adsorption reagent material, the radioactive wastewater can be treated. 60 Co. 90 Selective removal of Sr.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater treatment, and in particular to a preparation method and application of a cobalt and strontium selective adsorption reagent material. Background Art

[0002] 60 Co. 90 Sr is a common radionuclide in radioactive wastewater. 60 Co. 90 Sr exists mainly in the form of divalent ions in radioactive wastewater. Conventional ion exchange resins are used to treat radioactive wastewater containing Sr. 60 Co. 90 When Sr is used as radioactive wastewater, the non-radioactive divalent ion Ca in the wastewater 2+ Mg 2+ and 60 Co. 90 Sr forms a strong competition, resulting in the exchange capacity of the ion exchange resin being mainly occupied by Ca 2+ Mg 2+ In fact, for most selective adsorbents, the selectivity coefficient of strontium / calcium is in the range of 1 to 10. This low selectivity cannot ensure efficient treatment of strontium and cobalt in solutions with high salt content, which reduces the utilization efficiency of ion exchange resins and increases the amount of waste resin generated. Summary of the invention

[0003] The present invention provides a preparation method and application of a cobalt and strontium selective adsorption reagent material. The silicate material and the reagent are used in combination to significantly improve the material's ability to selectively adsorb cobalt and strontium in high-salinity radioactive wastewater. 60 Co. 90 The selectivity of Sr. The adsorption reagent material and SO4 in radioactive wastewater 2- PO4 3- 、CO3 2- Through the combined action of ion exchange and co-precipitation on the adsorption reagent material, the radioactive wastewater can be treated. 60 Co. 90 Selective removal of Sr.

[0004] The present invention solves the above technical problems as follows: A method for preparing a cobalt and strontium selective adsorption reagent material comprises the following steps:

[0005] 1) Fully mix silicon dioxide and sodium hydroxide in deionized water to prepare silica sol Na2O·nSiO2;

[0006] 2) Mix the silica sol Na2O·nSiO2 and the barium chloride solution, stir, let it stand and settle, remove the supernatant and filter, and obtain the amorphous barium silicate SiOx Ba and dry to obtain the adsorption reagent material.

[0007] Preferably, in step 1), the molar ratio of silicon dioxide to sodium hydroxide is 1:0.01-0.1. More preferably, in step 1), the molar ratio of silicon dioxide to sodium hydroxide is 1:0.05-0.08.

[0008] Preferably, in step 2), the mass concentration of the barium chloride solution is 5%.

[0009] Preferably, in step 2), the molar ratio of silicon dioxide to barium chloride is 1:0.2-1.5. More preferably, in step 2), the molar ratio of silicon dioxide to barium chloride is 1:0.3.

[0010] Preferably, in step 2), the stirring time is 2-4 hours, and the settling time is 20-30 hours. Further preferably, in step 2), the stirring time is 3 hours, and the settling time is 24 hours.

[0011] Preferably, in step 2), the drying temperature is 100-150°C, and the drying time is 20-30 hours. More preferably, in step 2), the drying temperature is 130°C, and the drying time is 24 hours.

[0012] The cobalt and strontium selective adsorption reagent material prepared by the method described above is used in treating radioactive wastewater.

[0013] In the above application, the radioactive wastewater contains 60 Co. 90 Sr, Ca 2+ Mg 2+ 、SO4 2- PO4 3- 、CO3 2- The cobalt and strontium selective adsorption reagent material provided by the present invention can be used in Ca 2+ Mg 2+ To achieve the radioactive wastewater treatment without interference 60 Co. 90 Selective removal of Sr. To further improve the adsorption effect, SO4 can also be added to the wastewater 2- PO4 3- 、CO3 2- Plasma promotes ion exchange and co-precipitation.

[0014] The working principle of the present invention is:

[0015] The active ingredient of the adsorption reagent material provided by the present invention is amorphous barium silicate SiO x Ba and SO4 in Radioactive Wastewater 2- PO43- 、CO3 2- Through the combined action of ion exchange and co-precipitation on the adsorption reagent material, the radioactive wastewater can be treated. 60 Co. 90 Selective removal of Sr.

[0016] The properties of this material are mainly affected by two factors:

[0017] (1) The size of n in silica sol Na2O·nSiO2 will affect the material bonding Ba 2+ The ability and structure of the final amorphous barium silicate affect the adsorption performance.

[0018] (2) The molar ratio of barium chloride solution and silica sol when mixed affects the amorphous barium silicate SiO x The size of x in Ba will affect the ion exchange ability and co-precipitation ability of the material.

[0019] The beneficial effects of the present invention are as follows: the present invention generates an adsorption reagent material by reacting silica sol with a soluble barium salt and is applied to selectively adsorb strontium and cobalt from radioactive wastewater. The preparation method provided by the present invention is simple, the raw materials are readily available, the reaction conditions are mild, the adsorption efficiency is high, and it has considerable promotion prospects.

[0020] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. The specific implementation of the present invention is given in detail by the following embodiments and their accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0022] Figure 1 is a graph showing the removal rate of the adsorbent material in Example 1 as a function of the sodium / silicon molar ratio;

[0023] Figure 2 Graph showing the removal rate of the adsorbent material in Example 1 as a function of the silicon / barium molar ratio. DETAILED DESCRIPTION

[0024] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0025] Example 1

[0026] This example provides a cobalt and strontium selective adsorption reagent material and explores the effects of the amounts of silicon, sodium and barium in the raw materials on the performance of the adsorption reagent material.

[0027] 1. Preparation method of adsorption reagent material

[0028] Silicon dioxide and sodium hydroxide are fully mixed in deionized water to prepare silica sol Na2O·nSiO2. By adjusting different masses of sodium hydroxide, silica sol Na2O·nSiO2 with different silicon-sodium molar ratios is prepared. Then, it is mixed with a certain amount of barium chloride solution with a mass concentration of 5%, stirred for 3 hours, and settled for 24 hours. The supernatant is skimmed off and filtered, and the resulting product is dried at 130°C for 24 hours to obtain an adsorption reagent material.

[0029] 2. Investigate the effect of silicon-sodium molar ratio on adsorption reagent materials

[0030] As shown in Table 1, the molar amount of barium in the raw material was fixed, and the molar ratio of silicon and sodium in the raw material was changed to explore the effect of the silicon-sodium ratio on the adsorption reagent material. Specifically, 0.02 g of the adsorption reagent material was put into a 150 mL conical flask, and 100 mL of simulated waste liquid was added. After that, it was shaken in a shock box for 24 hours. The concentrations of cobalt and strontium in the simulated waste liquid before and after treatment were measured by a flame atomic absorption spectrophotometer to test the performance of the adsorption reagent material. The results are as follows: Figure 1 As shown. Co in simulated wastewater 2+ , Sr 2+ The concentration is 5 mg / L, interfering ion Ca 2+ Mg 2+ The concentration is 50 mg / L and the sulfate concentration is 0.5 g / L.

[0031] Table 1 Molar ratio of silicon, barium and sodium in each group of adsorption reagent materials

[0032]

[0033] like Figure 1 As shown in the experimental range, with the increase of sodium-silicon molar ratio, the adsorption of Co by the adsorbent material 2+ , Sr 2+ The removal rate first increases and then decreases, and the optimal silicon-sodium molar ratio is between 1:0.05 and 1:0.08.

[0034] 2. Investigate the effect of silicon-barium molar ratio on adsorption reagent materials

[0035] As shown in Table 2, the molar amount of sodium in the raw material was fixed, and the molar ratio of silicon and barium in the raw material was changed to explore the effect of the silicon-barium ratio on the adsorption reagent material. Specifically, 0.02 g of the adsorption reagent material was put into a 150 mL conical flask, and 100 mL of simulated waste liquid was added. After that, it was shaken in a shock box for 24 hours. The concentrations of cobalt and strontium in the simulated waste liquid before and after treatment were measured by a flame atomic absorption spectrophotometer to test the performance of the adsorption reagent material. The results are as follows: Figure 2 As shown. Co in simulated wastewater 2+ , Sr 2+ The concentration is 5 mg / L, interfering ion Ca 2+ Mg 2+ The concentration is 50 mg / L and the sulfate concentration is 0.5 g / L.

[0036] Table 2 Molar ratios of silicon, barium and sodium in each group of adsorption reagent materials

[0037]

[0038] Depend on Figure 2 It can be seen that within the experimental range, when the molar ratio of silicon to barium is around 1:0.3 (i.e., 3.34), the adsorption of the reagent material to Co 2+ , Sr 2+ The removal rate reaches the maximum.

[0039] Example 2

[0040] This example uses the adsorption reagent material No. 3 in Example 1, with a silicon-barium-sodium molar ratio of 1:0.3:0.05, to test its adsorption of Sr under different sulfate concentration conditions. 2+ processing effect.

[0041] Preparation of Sr 2+ The concentration is 5 mg / L, interfering ion Ca 2+ Mg 2+ The concentration of the simulated waste liquid was 50 mg / L, and the sulfate concentration was 0.05, 0.1, 0.5, 1, and 5 g / L respectively. 0.05 g of the adsorption reagent material was placed in a 150 mL conical flask, and 100 mL of the simulated waste liquid was added. After that, it was shaken in a shaker for 24 hours. The strontium concentration in the simulated waste liquid before and after treatment was measured by a flame atomic absorption spectrophotometer to test its effect on Sr 2+ The results of the treatment are shown in Table 3.

[0042] Table 3 Effect of sulfate concentration on the adsorption of Sr by adsorption reagent materials 2+ The impact of the effect

[0043]

[0044] Example 3

[0045] This example uses the adsorption reagent material No. 3 in Example 1, with a silicon-barium-sodium molar ratio of 1:0.3:0.05, to test its adsorption of Sr under different oxalate concentration conditions. 2+ processing effect.

[0046] Preparation of Sr 2+ The concentration is 5 mg / L, interfering ion Ca 2+ Mg 2+ The concentration of the simulated waste liquid was 50 mg / L, and the oxalate concentration was 0.05, 0.1, 0.5, 1, and 5 g / L respectively. 0.05 g of the adsorption reagent material was placed in a 150 mL conical flask, and 100 mL of the simulated waste liquid was added. After that, it was shaken in a shaker for 24 hours. The strontium concentration in the simulated waste liquid before and after treatment was measured by a flame atomic absorption spectrophotometer to test its effect on Sr 2+ The results of the treatment are shown in Table 4.

[0047] Table 4 Effect of oxalate concentration on the adsorption of Sr by adsorption reagent materials 2+ The impact of the effect

[0048]

[0049] Example 4

[0050] This example uses the adsorption reagent material No. 3 in Example 1, with a silicon-barium-sodium molar ratio of 1:0.3:0.05, to test its adsorption of Co under different carbonate concentration conditions. 2+ , Sr 2+ processing effect.

[0051] Preparation of Sr 2+ The concentration is 5 mg / L, interfering ion Ca 2+ Mg 2+ The concentration of the simulated waste liquid was 50 mg / L, and the carbonate concentration was 1, 5, 10, 50, and 100 mg / L respectively. 0.05 g of the adsorption reagent material was placed in a 150 mL conical flask, and 100 mL of the simulated waste liquid was added. After that, it was shaken in a shaker for 24 hours. The strontium concentration in the simulated waste liquid before and after treatment was measured by a flame atomic absorption spectrophotometer to test its effect on Sr 2+ The results of the treatment are shown in Table 5.

[0052] Table 5 Effect of carbonate concentration on the adsorption of Sr by adsorption reagent materials 2+ The impact of the effect

[0053]

[0054] Formulated Co 2+ The concentration is 5 mg / L, interfering ion Ca 2+ Mg 2+The concentration of the simulated waste liquid was 50 mg / L, and the carbonate concentration was 1, 5, 10, 50, and 100 mg / L respectively. 0.05 g of the adsorption reagent material was placed in a 150 mL conical flask, and 100 mL of the simulated waste liquid was added. After that, it was shaken in a shaker for 24 hours. The strontium concentration in the simulated waste liquid before and after treatment was measured by a flame atomic absorption spectrophotometer to test its effect on Co 2+ The results of the treatment are shown in Table 6.

[0055] Table 6 Effect of carbonate concentration on the adsorption of Co by adsorbent materials 2+ The impact of the effect

[0056]

[0057] Example 5

[0058] This example uses the adsorption reagent material No. 3 in Example 1, with a silicon-barium-sodium molar ratio of 1:0.3:0.05, to test its adsorption of Co under different phosphate concentration conditions. 2+ , Sr 2+ processing effect.

[0059] Preparation of Sr 2+ The concentration is 5 mg / L, interfering ion Ca 2+ Mg 2+ The concentration of the simulated waste liquid was 50 mg / L, and the phosphate concentration was 1, 5, 10, 50, and 100 mg / L respectively. 0.05 g of the adsorption reagent material was placed in a 150 mL conical flask, and 100 mL of the simulated waste liquid was added. After that, it was shaken in a shaker for 24 hours. The strontium concentration in the simulated waste liquid before and after treatment was measured by a flame atomic absorption spectrophotometer to test its effect on Sr 2+ The results of the treatment are shown in Table 7.

[0060] Table 7 Effect of phosphate concentration on the adsorption of Sr by adsorption reagent materials 2+ The impact of the effect

[0061]

[0062] Formulated Co 2+ The concentration is 5 mg / L, interfering ion Ca 2+ Mg 2+ The concentration of strontium in the simulated waste liquid was 50 mg / L, and the phosphate concentration was 1, 5, 10, 50, and 100 mg / L respectively. 0.05 g of the adsorption reagent material was placed in a 150 mL conical flask, and 100 mL of the simulated waste liquid was added. After that, it was shaken in a shaker for 24 hours. The strontium concentration in the simulated waste liquid before and after treatment was measured by a flame atomic absorption spectrophotometer to test its effect on Co 2+ The results of the treatment are shown in Table 7.

[0063] Table 8 Effect of phosphate concentration on adsorption of Co by adsorption reagent materials 2+ The impact of the effect

[0064]

[0065] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as shown in the drawings and described above. However, any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a cobalt and strontium selective adsorption reagent material, It is characterized in that The following steps are involved: 1) Mix silicon dioxide and sodium hydroxide in deionized water to prepare silica sol Na 2 O·nSiO 2 ; 2) Silica sol Na 2 O·nSiO 2 After mixing with barium chloride solution, stirring and standing to settle, the supernatant was skimmed off and filtered to obtain the product, amorphous barium silicate SiO x Ba is dried at 100-150°C for 20-30 hours to obtain the adsorption reagent material; wherein the molar ratio of silicon dioxide to sodium hydroxide is 1:0.05-0.08; and the molar ratio of silicon dioxide to barium chloride is 1:0.

3.

2. A method for preparing a cobalt and strontium selective adsorption reagent material according to claim 1, It is characterized in that In the step 2), the mass concentration of the barium chloride solution is 5%.

3. A method for preparing a cobalt and strontium selective adsorption reagent material according to claim 1, It is characterized in that In the step 2), the stirring time is 2-4 h and the sedimentation time is 20-30 h.

4. Use of the cobalt and strontium selective adsorption reagent material prepared according to any one of claims 1 to 3 in treating radioactive wastewater.

5. The use according to claim 4, It is characterized in that The radioactive wastewater contains 60 Co. 90 Sr, Ca 2+ Mg 2 + 、SO 4 2- ,PO 4 3- , CO 3 2- .

Citation Information

Patent Citations

  • Composite flocculating agent for processing radioactive elements iron, cobalt, manganese and silver in nuclear waste water and processing method

    CN103151088A

  • Method for purifying sewage containing heavy metal by utilizing calcium metasilicate and recycling heavy metal

    CN104016434A

  • Strontium and cesium specific ion-exchange media

    CN109908858A

  • Decontamination agent for radioactive cesium and method of water depth-adjustable decontamination of radioactive cesium

    CN113164911A

  • Aluminosilicate amorphous material, its manufacturing method and material to remove heavy metal ion

    JP2004051457A