Composition for active layer, active layer, organic solar cell and preparation method thereof

CN117769269BActive Publication Date: 2024-11-26SHENZHEN POLYTECHNIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410015298.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-04
Publication Date
2024-11-26
Estimated Expiration
2044-01-04

AI Technical Summary

Technical Problem

The micromorphology of the active layer of organic solar cells is unstable, resulting in insufficient charge transport and extraction capabilities, affecting device efficiency and stability.

Method used

Using a composition including donor material and acceptor material, non-volatile additives are added to form conjugated surface stacking between molecules, adjust the morphological distribution, build a microcrystalline 'interleaved' morphological network, optimize the phase separation scale and crystallization improves micromorphic stability and charge transport capability.

Benefits of technology

It significantly improves the photoelectric conversion efficiency and stability of organic solar cells, reduces defects in the active layer, improves charge collection and extraction capabilities, and enhances the commercial potential of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117769269B_ABST
    Figure CN117769269B_ABST
Patent Text Reader

Abstract

The present invention discloses a composition for an active layer, an active layer, an organic solar cell and a preparation method thereof. The composition for an active layer comprises an active material and an additive, wherein the additive comprises at least one of the following structures: #imgabs0# The active material comprises a donor material and an acceptor material. When the composition of the present invention is used for an active layer, the non-volatile additive can form a conjugated surface stacking between molecules with the donor material and the acceptor material during the crystallization process, adjust the morphology distribution, optimize the phase separation scale, microscopic morphology scale and crystallinity in the active layer, and construct a morphology network of "interpenetrating" microcrystals to ensure a good and stable microscopic morphology structure, thereby improving the charge collection efficiency and the ability to extract electrons, reducing defects in the active layer to reduce trap-assisted recombination, effectively solving the problem of insufficient stability caused by morphology defects in the active layer, and effectively improving the efficiency and stability of the organic solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a composition for an active layer, an active layer, an organic solar cell and a preparation method thereof. Background Art

[0002] The excessive use of fossil energy and the increase in greenhouse gases caused by the rapid development of globalization have led to various environmental problems such as temperature change and sea level rise. The development of clean and renewable energy is the only way for the green economic cycle to develop. Among them, solar energy is the first choice for renewable clean energy, and thermal conversion and light conversion are the two most important strategies. The use of photoelectric conversion is currently the most mature solution, and silicon-based solar cells are the main representative. However, silicon-based solar cells are limited in their diversified development due to problems such as hard materials, large environmental and spatial utilization ranges, etc.

[0003] Organic solar cells have great development potential in the fields of indoor photovoltaics and wearables due to their advantages such as low raw material cost, light weight and flexibility. The micromorphology of the active layer of organic solar cells directly determines the photoelectric conversion efficiency of organic solar cells. How to regulate the micromorphology of the active layer to improve the photoelectric conversion efficiency of organic solar cells is a problem that must be solved on the road to commercialization. The micromorphology of the active layer can be effectively regulated by the additive strategy, but the volatility of the additive causes the micromorphology structure to be in a metastable state, resulting in defects in the domain size structure and increased recombination. There is still a great risk to the efficiency and stability of the device. Solving the defects in the domain size structure and the deficiencies in charge transfer and extraction will help promote the further development of organic solar cells.

[0004] In view of this, it is of great practical significance to seek an external additive that can effectively improve the morphology of the active layer of organic solar cells, enhance the stability of the microscopic morphology, and at the same time permanently and stably enhance the charge transfer and extraction capabilities. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a composition for an active layer, an active layer, an organic solar cell and a preparation method thereof, aiming to improve the microscopic morphology stability of the active layer of the organic solar cell and improve the charge transfer and extraction capabilities.

[0006] The technical solution of the present invention is as follows:

[0007] In a first aspect of the present invention, a composition for an active layer is provided, wherein the composition for an active layer comprises an active material and an additive, and the additive comprises at least one of the following structures:

[0008]

[0009] The active material includes a donor material and an acceptor material.

[0010] Optionally, the ratio of the total mass of the donor material and the acceptor material to the mass of the additive is 15.4:(1.5-2.5).

[0011] Optionally, the donor material comprises at least one of the following structures:

[0012]

[0013] in, represents the connection site,

[0014] Optionally, the receptor material comprises at least one of the following structures:

[0015]

[0016] A second aspect of the present invention provides an active layer, wherein the active layer comprises the composition for an active layer as described above.

[0017] According to a third aspect of the present invention, an organic solar cell is provided, wherein the organic solar cell comprises a first electrode layer, an active layer and a second electrode layer stacked in sequence, the active layer comprises the composition for an active layer as described above in the present invention, or the active layer comprises the active layer as described above in the present invention.

[0018] Optionally, the organic solar cell further comprises:

[0019] a hole transport layer disposed between the active layer and the first electrode layer;

[0020] An electron transport layer is disposed between the active layer and the second electrode layer.

[0021] A fourth aspect of the present invention provides a method for preparing the organic solar cell as described above, comprising the steps of:

[0022] providing a first electrode layer;

[0023] forming an active layer on the first electrode layer;

[0024] forming a second electrode layer on the active layer to obtain the organic solar cell; or,

[0025] providing a second electrode layer;

[0026] forming an active layer on the second electrode layer;

[0027] A first electrode layer is formed on the active layer to obtain the organic solar cell.

[0028] Optionally, the step of forming an active layer specifically includes:

[0029] Adding donor material, acceptor material and additive into a solvent to form an active material mixed solution;

[0030] The active material mixed solution is coated on the first electrode layer or the second electrode layer to obtain the active layer.

[0031] Optionally, in the active material mixed solution, the concentration of the additive is 1.5-2.5 mg / L;

[0032] And / or, the coating method is spin coating, drop coating or blade coating.

[0033] Beneficial effects: When the composition described in the present invention is used for the active layer, the non-volatile additive can form intermolecular conjugated surface stacking with the donor material and the acceptor material during the crystallization process, adjust the morphology distribution, optimize the phase separation scale, microscopic morphology scale and crystallinity in the active layer, and construct a morphology network of "interlaced" microcrystals to ensure a good and stable microscopic morphology structure, thereby improving the charge collection efficiency and the ability to extract electrons, enhancing the charge transfer capacity, reducing defects in the active layer and reducing trap-assisted recombination, effectively solving the problem of insufficient stability caused by morphology defects in the active layer, and effectively improving the efficiency and stability of organic solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Schematic diagram of the structure of the organic solar cell in Example 1 of the present invention.

[0035] Figure 2 (a) is a morphology diagram of the active layer in Example 1 of the present invention, and (b) is a morphology diagram of the active layer in Comparative Example 1 of the present invention.

[0036] Figure 3 Graph showing the stability test results of the organic solar cells in Example 2 of the present invention and Comparative Example 1.

[0037] Figure 4 1 is a graph showing the current density-voltage characteristic curves of the organic solar cells in Example 2 of the present invention and Comparative Example 1.

[0038] Figure 5 This is a graph showing the external quantum efficiency results of the organic solar cells in Example 2 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0039] The present invention provides a composition for an active layer, an active layer, a solar cell and a preparation method thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0040] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0041] An embodiment of the present invention provides a composition for an active layer, wherein the composition for an active layer includes an active material and an additive, and the additive includes at least one of the following structures:

[0042]

[0043] The active material includes a donor material and an acceptor material.

[0044] When the composition described in the present invention is used in the active layer, the non-volatile additive can form intermolecular conjugated surface stacking with the donor material and the acceptor material during the crystallization process, adjust the morphology distribution, optimize the phase separation scale, microscopic morphology scale and crystallinity in the active layer, and construct a morphology network of "interlaced" microcrystals to ensure a good and stable microscopic morphology structure, thereby improving the charge collection efficiency and the ability to extract electrons, enhancing the charge transfer capacity, reducing defects in the active layer, reducing trap-assisted recombination, and effectively solving the problem of insufficient stability caused by morphology defects in the active layer, effectively improving the efficiency and stability of organic solar cells. The composition described in the present invention has great commercial potential in the future industrialization process of organic solar cells, and is expected to tap the greater potential of existing materials.

[0045] In some embodiments, the ratio of the total mass of the donor material and the acceptor material to the mass of the additive is 15.4:(1.5-2.5). For example, the ratio is 15.4:1.5, 15.4:2, 15.4:2.2, or 15.4:2.5.

[0046] The present invention does not limit the types of specific donor materials and acceptor materials. As an example, in some embodiments, the donor material includes at least one of the following structures:

[0047]

[0048] Where n is the degree of polymerization, Indicates the connection site.

[0049] In some embodiments, the receptor material comprises at least one of the following structures:

[0050]

[0051]

[0052] The embodiment of the present invention further provides an active layer, wherein the active layer comprises the composition for active layer as described above in the embodiment of the present invention. That is, the active layer comprises a donor material, an acceptor material and an additive. The selection of the donor material, the acceptor material and the additive is as described above.

[0053] In the active layer provided by the embodiment of the present invention, the non-volatile additive can form intermolecular conjugated surface stacking with the donor material and the acceptor material during the crystallization process, adjust the morphology distribution, optimize the phase separation scale, microscopic morphology scale and crystallinity in the active layer, and the constructed microcrystal "interlaced" morphology network can ensure that a good and stable microscopic morphology structure is obtained. At the same time, the formation of the microcrystalline morphology can improve the charge transmission channel, improve the charge collection efficiency and the ability to extract electrons, enhance the charge transmission capacity, reduce defects in the active layer, reduce trap-assisted recombination, and effectively solve the problem of insufficient stability caused by morphology defects in the active layer. The composition of the present invention can effectively improve the efficiency and stability of organic solar cells, has great commercial potential in the future industrialization process of organic solar cells, and is expected to tap the greater potential of existing materials.

[0054] An embodiment of the present invention further provides an organic solar cell, wherein the organic solar cell comprises a first electrode layer, an active layer and a second electrode layer stacked in sequence, the active layer comprises the composition for an active layer as described above in the tenth embodiment of the present invention, or the active layer comprises the active layer as described above in the embodiment of the present invention.

[0055] In some embodiments, the thickness of the active layer is 90-110 nm. For example, the thickness of the active layer is 90 nm, 92 nm, 95 nm, 98 nm, 100 nm, 102 nm, 105 nm, 107 nm, 108 nm or 110 nm.

[0056] The organic solar television provided by the embodiment of the present invention has higher efficiency and stability.

[0057] In some embodiments, the organic solar cell further comprises:

[0058] a hole transport layer disposed between the active layer and the first electrode layer;

[0059] An electron transport layer is disposed between the active layer and the second electrode layer.

[0060] In some embodiments, the thickness of the hole transport layer is 30-40 nm. For example, the thickness of the hole transport layer is 30 nm, 32 nm, 34 nm, 35 nm, 36 nm, 38 nm or 40 nm.

[0061] In some embodiments, the thickness of the electron transport layer is 5-12 nm. For example, the thickness of the electron transport layer is 5 nm, 8 nm, 10 nm or 12 nm.

[0062] The present invention does not limit the materials of the hole transport layer and the electron transport layer, and any hole transport material and electron transport material are applicable to the present invention. As an example, the hole transport material is PEDOT:PSS, and the electron transport material is selected from at least one of the following structures:

[0063]

[0064] The present invention also provides a method for preparing the organic solar cell according to the present invention, which comprises the following steps:

[0065] S11, providing a first electrode layer;

[0066] S12, forming an active layer on the first electrode layer;

[0067] S13, forming a second electrode layer on the active layer to obtain the organic solar cell; or,

[0068] S21, providing a second electrode layer;

[0069] S22, forming an active layer on the second electrode layer;

[0070] S23, forming a first electrode layer on the active layer to obtain the organic solar cell.

[0071] In steps S22 and S23, in some embodiments, the step of forming an active layer specifically includes:

[0072] Adding donor material, acceptor material and additive into a solvent to form an active material mixed solution;

[0073] The active material mixed solution is coated on the first electrode layer or the second electrode layer to obtain the active layer.

[0074] In some embodiments, in the active material mixed solution, the concentration of the additive is 1.5-2.5 mg / L. For example, the concentration of the additive is 1.5 mg / L, 1.6 mg / L, 1.7 mg / L, 1.8 mg / L, 1.9 mg / L, 2.0 mg / L, 2.1 mg / L, 2.2 mg / L, 2.3 mg / L, 2.4 mg / L or 2.5 mg / L.

[0075] In some embodiments, the coating is performed by spin coating, drop coating or blade coating.

[0076] In some embodiments, the solvent includes at least one of chloroform, chlorobenzene, and o-xylene, but is not limited thereto.

[0077] In some embodiments, the organic solar cell further comprises: a hole transport layer disposed between the active layer and the first electrode layer and an electron transport layer disposed between the active layer and the second electrode layer. In this case, the method for preparing the organic solar cell specifically comprises the steps of:

[0078] S31, providing a first electrode layer;

[0079] S32, forming a hole transport layer on the first electrode layer;

[0080] S33, forming an active layer on the hole transport layer (specifically, coating an active material mixed solution on the hole transport layer);

[0081] S34, forming an electron transport layer on the active layer;

[0082] S35, forming a second electrode layer on the electron transport layer.

[0083] The following describes it in detail through specific embodiments.

[0084] The structural formula of the additive 1-HMB-Cl used in the following examples is The structural formula of the additive 2-HMB-Cl is Unless otherwise specified in the following examples, the raw materials used are all commercially available products.

[0085] Example 1

[0086] This embodiment provides an organic solar cell and a method for preparing the same. Figure 1 As shown, the organic solar cell includes an ITO conductive electrode layer, a hole transport layer (PEDOT:PSS), an active layer (corresponding to the Active Layer in the figure), an electron transport layer (PDINN) and an Ag electrode layer which are stacked in sequence.

[0087] The method for preparing the organic solar cell comprises the following steps:

[0088] Conductive glass (i.e., composed of a transparent substrate layer and a transparent ITO conductive electrode layer) with a surface roughness of less than 1 nm is ultrasonically cleaned with a cleaning solution, deionized water, acetone, and isopropanol, respectively, and then dried with nitrogen gas;

[0089] After the conductive glass was placed in an ozone cleaning machine for 20 minutes, a hole transport material solution (i.e., PEDOT:PSS, whose model is CLEVIOS P VP AI 4083) was spin-coated (7500 rpm, 30 seconds) on the ITO conductive electrode layer in air, and then thermally annealed at 150° C. in air for 10 minutes to form a hole transport layer with a thickness of 35 nm;

[0090] The sample was then placed in a glove box filled with nitrogen, and an active material mixed solution (containing 1.5 mg / mL of additive 1-HMB-Cl, 7 mg / L of PM6, 8.4 mg / L of BTP-ec9, and the solvent was o-xylene) was spin-coated on the hole transport layer (3500 rpm, 30 s), and then thermally annealed at 80 °C in the glove box for 5 min to form an active layer with a thickness of 100 nm;

[0091] Spin coating (2500 rpm, 20 s) an electron transport material solution (PDINN concentration is 2 mg / mL, the solvent can be methanol, ethanol or isopropanol, methanol is selected in this embodiment) on the active layer to form an electron transport layer with a thickness of 10 nm;

[0092] Then, Ag was evaporated on the electron transport layer to form an Ag electrode layer with a thickness of 100 nm, thereby obtaining the organic solar cell.

[0093] Example 2

[0094] The present embodiment provides an organic solar cell and a preparation method thereof. The organic solar cell includes an ITO conductive electrode layer, a hole transport layer (PEDOT:PSS), an active layer, an electron transport layer (PDINN) and an Ag electrode layer which are stacked in sequence.

[0095] The method for preparing the organic solar cell comprises the following steps:

[0096] Conductive glass (i.e., composed of a transparent substrate layer and a transparent ITO conductive electrode layer) with a surface roughness of less than 1 nm is ultrasonically cleaned with a cleaning solution, deionized water, acetone, and isopropanol, respectively, and then dried with nitrogen gas;

[0097] After the conductive glass was placed in an ozone cleaning machine for 20 minutes, a hole transport material solution (i.e., PEDOT:PSS, whose model is CLEVIOS P VP AI 4083) was spin-coated (7500 rpm, 30 seconds) on the ITO conductive electrode layer in air, and then thermally annealed at 150° C. in air for 10 minutes to form a hole transport layer with a thickness of 35 nm;

[0098] The sample was then placed in a glove box filled with nitrogen, and an active material mixed solution (containing 2 mg / mL of additive 1-HMB-Cl, 7 mg / L of PM6, 8.4 mg / L of BTP-ec9, and the solvent was o-xylene) was spin-coated on the hole transport layer (3500 rpm, 30 s), and then thermally annealed at 80 °C in the glove box for 5 min to form an active layer with a thickness of 100 nm;

[0099] An electron transport material solution (PDINN concentration of 2 mg / mL, solvent of methanol) was spin-coated (2500 rpm, 20 s) on the active layer to form an electron transport layer with a thickness of 10 nm;

[0100] Then, Ag was evaporated on the electron transport layer to form an Ag electrode layer with a thickness of 100 nm, thereby obtaining the organic solar cell.

[0101] Example 3

[0102] The present embodiment provides an organic solar cell and a preparation method thereof. The organic solar cell includes an ITO conductive electrode layer, a hole transport layer (PEDOT:PSS), an active layer, an electron transport layer (PDINN) and an Ag electrode layer which are stacked in sequence.

[0103] The method for preparing the organic solar cell comprises the following steps:

[0104] Conductive glass (i.e., composed of a transparent substrate layer and a transparent ITO conductive electrode layer) with a surface roughness of less than 1 nm is ultrasonically cleaned with a cleaning solution, deionized water, acetone, and isopropanol, respectively, and then dried with nitrogen gas;

[0105] After the conductive glass was placed in an ozone cleaning machine for 20 minutes, a hole transport material solution (i.e., PEDOT:PSS, whose model is CLEVIOS P VP AI 4083) was spin-coated (7500 rpm, 30 seconds) on the ITO conductive electrode layer in air, and then thermally annealed at 150° C. in air for 10 minutes to form a hole transport layer with a thickness of 35 nm;

[0106] The sample was then placed in a nitrogen-filled glove box, and an active material mixed solution (containing 2.5 mg / mL of additive 1-HMB-Cl, 7 mg / L of PM6, 8.4 mg / L of BTP-ec9, and the solvent was o-xylene) was spin-coated on the hole transport layer (3500 rpm, 30 s), and then thermally annealed at 80 °C in the glove box for 5 min to form an active layer with a thickness of 100 nm;

[0107] An electron transport material solution (PDINN concentration of 2 mg / mL, solvent of methanol) was spin-coated (2500 rpm, 20 s) on the active layer to form an electron transport layer with a thickness of 10 nm;

[0108] Then, Ag was evaporated on the electron transport layer to form an Ag electrode layer with a thickness of 100 nm, thereby obtaining the organic solar cell.

[0109] Example 4

[0110] The present embodiment provides an organic solar cell and a preparation method thereof. The organic solar cell includes an ITO conductive electrode layer, a hole transport layer (PEDOT:PSS), an active layer, an electron transport layer (PDINN) and an Ag electrode layer which are stacked in sequence.

[0111] The method for preparing the solar cell comprises the following steps:

[0112] Conductive glass (i.e., composed of a transparent substrate layer and a transparent ITO conductive electrode layer) with a surface roughness of less than 1 nm is ultrasonically cleaned with a cleaning solution, deionized water, acetone, and isopropanol, respectively, and then dried with nitrogen gas;

[0113] After the conductive glass was placed in an ozone cleaning machine for 20 minutes, a hole transport material solution (i.e., PEDOT:PSS, whose model is CLEVIOS P VP AI 4083) was spin-coated (7500 rpm, 30 seconds) on the ITO conductive electrode layer in air, and then thermally annealed at 150° C. in air for 10 minutes to form a hole transport layer with a thickness of 35 nm;

[0114] The sample was then placed in a glove box filled with nitrogen, and an active material mixed solution (containing 2.5 mg / mL of additive 2-HMB-Cl, 7 mg / L of PM6, 8.4 mg / L of BTP-ec9, and the solvent was o-xylene) was spin-coated on the hole transport layer (3500 rpm, 30 s), and then thermally annealed at 80 °C in the glove box for 5 min to form an active layer with a thickness of 100 nm;

[0115] An electron transport material solution (PDINN concentration of 2 mg / mL, solvent of methanol) was spin-coated (2500 rpm, 20 s) on the active layer to form an electron transport layer with a thickness of 10 nm;

[0116] Then, Ag was evaporated on the electron transport layer to form an Ag electrode layer with a thickness of 100 nm, thereby obtaining the solar cell.

[0117] Comparative Example 1

[0118] This comparative example provides an organic solar cell and a preparation method thereof. The organic solar cell includes an ITO conductive electrode layer, a hole transport layer (PEDOT:PSS), an active layer, an electron transport layer (PDINN) and an Ag electrode layer which are stacked in sequence.

[0119] The method for preparing the organic solar cell is different from that of Example 1 only in that the active material mixed solution does not contain the additive 1-HMB-Cl.

[0120] test:

[0121] (1) The microscopic morphology of the active layer in Example 1 and Comparative Example 1 is as follows Figure 2 As shown, it can be seen that there is no crystal phenomenon in the active layer of Comparative Example 1 (without additives), while the active layer in Example 1 has a crystalline structure, forming an "interspersed" morphology network of microcrystals. The "interspersed" morphology network of microcrystals can improve the stability of the active layer, while improving the charge transmission channel and transmission performance, thereby improving the charge extraction and collection efficiency of the active layer.

[0122] (2) The stability test results of the organic solar cells in Example 2 and Comparative Example 1 are as follows: Figure 3 As shown, it can be seen that the organic solar cell containing the active layer provided by the present invention has good stability and high photoelectric conversion efficiency. This fully proves that adding the additive provided by the present invention to the active layer can improve the stability and photoelectric conversion efficiency of the organic solar cell. The reason is that the scale of the microscopic morphology is mainly affected by the intermolecular stacking of the donor material and the acceptor material. The higher the molecular stacking degree and the more stable it is, the higher the efficiency of the organic solar cell will be, and the stability will be enhanced. In the present invention, the additive forms intermolecular conjugate surface stacking with the donor material and the acceptor material molecules in the active layer during the crystallization process, thereby adjusting the morphology distribution, and at the microscopic morphology scale, ensuring the high stacking degree and stability of the donor material and the acceptor material molecules, thereby improving the efficiency and stability of the organic solar cell.

[0123] (3) Under standard test conditions (AM1.5, 100mW / cm 2 ) The organic solar cells prepared in Examples 1-4 and Comparative Example 1 were tested, and the results were as follows Figure 4 , Figure 5 As shown in Table 1 below.

[0124] Table 1. Test results

[0125] Example <![CDATA[V oc (in)]]> <![CDATA[J sc (mA / cm 2 )]]> FF(%) PCE(%) Example 1 0.862 27.75 75.20 18.00 Example 2 0.865 27.82 75.56 18.28 Example 3 0.855 27.85 75.26 18.02 Example 4 0.854 27.70 75.17 17.78 Comparative Example 1 0.875 26.01 72.28 16.45

[0126] Among them, V oc is the open circuit voltage, J sc is the short-circuit current density, FF is the fill factor, and PCE is the photoelectric conversion efficiency.

[0127] From the results in Table 1, it can be seen that compared with the comparative example (the active layer does not contain additives), the organic solar cell provided by the embodiment of the present invention has higher short-circuit current density, fill factor and photoelectric conversion efficiency. It can be shown that by adding the additive to the active layer, the ability to extract charges can be effectively improved, the charge extraction efficiency can be improved (the improvement of short-circuit current density and fill factor indicates the improvement of charge extraction ability and charge extraction efficiency), thereby improving the efficiency of organic solar cells. The reason is that the addition of additives causes the active layer to form a microscopic morphology of "interpenetrating" microcrystals, thereby improving the charge transmission performance and transmission channel.

[0128] Figure 4 is a current density-voltage characteristic curve of the organic solar cell prepared in Example 2 and Comparative Example 1, Figure 5 Graphs showing the external quantum efficiency of the organic solar cells prepared in Example 2 and Comparative Example 1. Figure 4 and Figure 5 It can be seen that in the present invention, the current density and external quantum efficiency (EQE) of the solar cell can be improved by adding additives to the active layer.

[0129] In summary, the present invention provides a composition for an active layer, an active layer, a solar cell and a preparation method thereof, and specifically provides a simple, effective and universal external additive regulation strategy, namely, by introducing the above-mentioned non-volatile additives to regulate the morphology of the active layer, construct a microcrystal "interpenetrating" morphology network, optimize the phase separation scale and molecular stacking and crystallinity in the active layer, improve the microscopic morphology stability while improving the exciton dissociation ability and charge collection efficiency, and at the same time, the constructed microcrystal "interpenetrating" network effectively reduces the defects in the active layer morphology and reduces trap-assisted recombination, thereby improving the short-circuit current density of the organic solar cell while achieving the improvement of the efficiency and stability of the organic solar cell.

[0130] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A composition for an active layer, It is characterized in that The composition for the active layer is composed of an active material and an additive, wherein the additive comprises at least one of the following structures: ; The active material includes a donor material and an acceptor material.

2. The composition for active layer according to claim 1, It is characterized in that The ratio of the total mass of the donor material and the acceptor material to the mass of the additive is 15.4:(1.5-2.5).

3. The composition for active layer according to claim 1, It is characterized in that The donor material comprises at least one of the following structures: 、 、 ,in," " indicates the connection site, .

4. The composition for active layer according to claim 1, It is characterized in that The receptor material comprises at least one of the following structures: 、 、 、 。 5. An active layer, It is characterized in that The active layer comprises the composition for an active layer according to any one of claims 1 to 4.

6. An organic solar cell, It is characterized in that The organic solar cell comprises a first electrode layer, an active layer and a second electrode layer which are stacked in sequence, the active layer comprises the composition for an active layer according to any one of claims 1 to 4, or the active layer comprises the active layer according to claim 5.

7. The organic solar cell according to claim 6, It is characterized in that The organic solar cell further comprises: a hole transport layer disposed between the active layer and the first electrode layer; An electron transport layer is disposed between the active layer and the second electrode layer.

8. A method for preparing an organic solar cell as claimed in claim 6, It is characterized in that Includes steps: providing a first electrode layer; forming an active layer on the first electrode layer; forming a second electrode layer on the active layer to obtain the organic solar cell; or, providing a second electrode layer; forming an active layer on the second electrode layer; A first electrode layer is formed on the active layer to obtain the organic solar cell.

9. The preparation method according to claim 8, It is characterized in that The step of forming the active layer specifically includes: Adding donor material, acceptor material and additive into a solvent to form an active material mixed solution; The active material mixed solution is coated on the first electrode layer or the second electrode layer to obtain the active layer.

10. The preparation method according to claim 9, It is characterized in that In the active material mixed solution, the concentration of the additive is 1.5-2.5 mg / L; And / or, the coating method is spin coating, drop coating or blade coating.

11. Use of the composition for active layer according to any one of claims 1 to 4 in improving the microscopic morphology stability, charge transport capability and charge extraction capability of the active layer of an organic solar cell.