Amphoteric perfluorosulfonic acid ion exchange membrane and its preparation method and application

By using the casting method and graft modification technology in the vanadium battery membrane material, an amphoteric perfluorosulfonic acid ion exchange membrane was prepared, which solved the problem of balancing the conductivity and vanadium ion permeability of the vanadium battery membrane material, and significantly improved the vanadium Overall performance of battery separators.

CN117777508BActive Publication Date: 2024-10-29THINKRE MEMBRANE MATERIAL
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311769500.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-21
Publication Date
2024-10-29
Estimated Expiration
2043-12-21

AI Technical Summary

Technical Problem

Existing vanadium battery membrane materials are difficult to effectively reduce the permeability of vanadium ions while improving conductivity, resulting in insufficient comprehensive performance of the vanadium battery separator.

Method used

The amphoteric perfluorosulfonic acid ion exchange membrane was prepared by the casting method, and the perfluorosulfonic acid fluororesin was grafted and modified by anionic and cationic irradiation with the grafting aid p-fluorostyrene to increase the grafting rate, and through sodium and Hydrogenation treatment produces a membrane material with evenly distributed anions and cations, reducing the permeability of vanadium ions.

Benefits of technology

It is possible to significantly reduce the permeability of vanadium ions while maintaining good electrical conductivity, and improve the comprehensive performance of the vanadium battery separator.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an amphoteric perfluorosulfonic acid ion exchange membrane and a preparation method and application thereof. The preparation method comprises the following steps: (1) fully mixing raw materials including perfluorosulfonic acid fluorine resin powder, anion modifier, cationic modifier and grafting auxiliary agent in a reaction kettle in proportion, adding solvent, excluding gas and filling with inert gas and sealing, heating to 100-105°C, completely dissolving the raw materials, gamma ray irradiation, irradiation dose 3-3.5Mrad, cooling to room temperature, and obtaining a grafted mixed liquid; (2) drying and concentrating the grafted mixed liquid to obtain a mother liquor; (3) scraping the mother liquor on a substrate, and drying to obtain a primary membrane; (4) subjecting the primary membrane to gamma ray irradiation treatment to obtain a treated membrane; (5) subjecting the treated membrane to sodiumization and hydrogenation to obtain an anionic and cationic perfluorosulfonic acid ion exchange membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an amphoteric perfluorosulfonic acid ion exchange membrane and a preparation method and application thereof, belonging to the field of vanadium battery ion exchange membranes. Background Art

[0002] Compared with other energy storage batteries, vanadium redox flow batteries (VRBs) have the characteristics of high energy efficiency, short response time, low self-discharge rate, and long cycle life, and therefore have attracted widespread attention and application. Vanadium redox flow batteries are considered to be a highly efficient energy storage / conversion system. Their design capacity is much larger than that of conventional batteries, and they have obvious advantages. They can be connected to the power system on a large scale and are widely used in large-scale energy storage devices such as load balancing, grid peak regulation, and uninterruptible power supplies (UPS).

[0003] At present, as one of the key components of redox flow batteries, membrane materials are used to separate positive and negative half-cells, and also need to provide channels for charge-balancing ions to ensure the battery circuit. In recent years, basic research and industrial application research on membrane materials for vanadium batteries have received widespread attention and have made great progress. According to different mechanisms, membrane materials for vanadium batteries can be divided into cation exchange membranes (CEM), anion exchange membranes (AEMS), amphoteric ion exchange membranes (ALEM) and porous membranes. The resin material of Nafion membrane is sulfonated tetrafluoroethylene polymer, which has high conductivity and is the most widely used cation exchange membrane material, but the vanadium permeability is large; while the anion exchange membrane reduces the permeation of vanadium ions due to the Donnan exclusion effect, but is also limited by low conductivity; therefore, the research direction in this field is to prepare amphoteric ion exchange membranes with both high conductivity and low vanadium ion permeability in a method suitable for mass production. Summary of the invention

[0004] In view of the problems existing in the background technology, the purpose of the present invention is to provide an amphoteric perfluorosulfonic acid ion exchange membrane and a preparation method thereof, wherein the grafting auxiliary agent p-fluorostyrene is used to efficiently and uniformly graft anions and cations on the perfluorosulfonic acid fluorine resin by irradiation grafting, and then the amphoteric perfluorosulfonic acid resin prepared by the method has anions and cations uniformly distributed on the whole, and the grafting rate is improved; the above-mentioned modified raw materials are used to prepare an ion exchange membrane for vanadium batteries by a casting film method, not only the anions maintain a good conductivity of the film, but also the Donnan exclusion effect of the cations reduces the penetration of vanadium ions, improves the barrier property of vanadium ions, and greatly improves the comprehensive performance of the vanadium battery separator.

[0005] In order to achieve the above-mentioned object, the present invention provides a method for preparing an amphoteric perfluorosulfonic acid ion exchange membrane by a casting method, comprising the following steps: (1) fully mixing raw materials including perfluorosulfonic acid fluorine resin powder, anion modifier, cation modifier and grafting auxiliary agent in a reaction kettle in proportion, adding a solvent, removing gas and filling with inert gas and then sealing, heating to 100-105° C. to completely dissolve the raw materials, irradiating with gamma rays with an irradiation dose of 3-3.5 Mrad, cooling to room temperature, and obtaining a grafted mixed liquid; (2) drying and concentrating the grafted mixed liquid described in step (1) to obtain a mother liquor; (3) scraping the mother liquor described in step (2) on a substrate, and drying to obtain a primary membrane; (4) subjecting the primary membrane described in step (3) to gamma ray irradiation treatment to obtain a treated membrane; (5) subjecting the treated membrane described in step (4) to sodiumization and hydrogenation to obtain an anionic and cationic perfluorosulfonic acid ion exchange membrane.

[0006] Optionally, the anion modifier is one or a combination of styrene sulfonic acid, sodium styrene sulfonate and 3-sulfonyl methacrylate.

[0007] Optionally, the cationic modifier is one or a combination of dimethylaminoethyl methacrylate, N-(4-vinylbenzyl)-N,N-dialkylamine, N-isopropylacrylamide, methacryloyloxyethyltrimethylammonium chloride and 1-allyl-3-vinylimidazole acetate.

[0008] Optionally, the grafting aid is p-fluorostyrene.

[0009] Optionally, the solvent is one of N-methylpyrrolidone, dimethyl sulfoxide and N,N-dimethylformamide.

[0010] Optionally, the mass ratio of perfluorosulfonic acid fluorine-type resin powder, anion modifier, cationic modifier, grafting aid and solvent is 100:(4-5):(6-9):(1-1.5):(1000-2000).

[0011] Optionally, the number of times of excluding gas and filling in inert gas in step (2) is 3-5 times; the inert gas is nitrogen or argon.

[0012] Optionally, the sodiumization and hydrogenation in step (5) are specifically carried out by sequentially sodiumizing the treated membrane in step (4) with a 25wt% NaOH methanol solution and hydrogenating it with a 16wt% hydrochloric acid solution, washing it with deionized water, and drying it to obtain an amphoteric perfluorosulfonic acid ion exchange membrane.

[0013] The invention also provides an amphoteric perfluorosulfonic acid ion exchange membrane prepared by the method described above.

[0014] The invention also provides an application of an amphoteric perfluorosulfonic acid ion exchange membrane, wherein the amphoteric perfluorosulfonic acid ion exchange membrane is used for a vanadium battery.

[0015] The beneficial effects of the present invention are as follows:

[0016] 1. In the present application, after completely dissolving the perfluorosulfonic acid fluororesin, anion modifier, cation modifier and grafting aid by solvent, the resin is activated by gamma ray irradiation in a closed reactor under the protection of inert gas under heating. The grafting aid plays an auxiliary role in grafting specific anion and cation modifiers onto the molecular chain of the perfluorosulfonic acid fluororesin, thereby increasing the branching degree of the perfluorosulfonic acid fluororesin and providing it with suitable viscoelasticity, which facilitates the preparation of amphoteric perfluorosulfonic acid ion exchange membrane with excellent comprehensive performance by film casting.

[0017] 2. The graft-modified casting mother solution of the present invention has good film-forming properties. The prepared amphoteric perfluorosulfonic acid ion exchange membrane has uniform thickness and a smooth surface. The amphoteric ion exchange membrane significantly reduces the permeability of vanadium ions while maintaining good conductivity. DETAILED DESCRIPTION

[0018] In order to make the above-mentioned objects, features and advantages of the invention more obvious and easy to understand, the specific embodiments of the invention are described in detail below.

[0019] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0020] The method for preparing amphoteric perfluorosulfonic acid ion exchange membrane by a casting method according to the present invention comprises the following steps: (1) fully mixing raw materials including perfluorosulfonic acid fluorine resin powder, anion modifier, cation modifier and grafting aid in a reaction kettle in proportion, adding solvent, removing gas and filling with inert gas and then sealing, heating to 100-105° C. to completely dissolve the raw materials, irradiating with gamma rays with an irradiation dose of 3-3.5 Mrad, cooling to room temperature, and obtaining a grafted mixed liquid; (2) drying and concentrating the grafted mixed liquid described in step (1) to obtain a mother liquor; (3) applying the mother liquor described in step (2) on a substrate and drying to obtain a primary membrane; (4) subjecting the primary membrane described in step (3) to gamma ray irradiation treatment to obtain a treated membrane; (5) subjecting the treated membrane described in step (4) to sodiumization and hydrogenation to obtain an anionic and cationic perfluorosulfonic acid ion exchange membrane. The anion modifier is one or a combination of styrene sulfonic acid, sodium styrene sulfonate and 3-sulfonyl methacrylate. The cationic modifier is one or a combination of dimethylaminoethyl methacrylate, N-(4-vinylbenzyl)-N,N-dialkylamine, N-isopropylacrylamide, methacryloyloxyethyl trimethylammonium chloride and 1-allyl-3-vinyl imidazole acetate. The grafting aid is p-fluorostyrene. The solvent is one of N-methylpyrrolidone, dimethyl sulfoxide and N,N-dimethylformamide.

[0021] In the method for preparing amphoteric perfluorosulfonic acid ion exchange membrane by the casting method according to the present invention, the mass ratio of perfluorosulfonic acid fluorine-type resin powder, anion modifier, cationic modifier, grafting aid and solvent is 100:(4-5):(6-9):(1-1.5):(1000-2000).

[0022] In the method for preparing amphoteric perfluorosulfonic acid ion exchange membrane by the casting method according to the present invention, the number of times of exhausting gas and filling in inert gas in step (2) is 3-5 times; the inert gas is nitrogen or argon.

[0023] In the method for preparing an amphoteric perfluorosulfonic acid ion exchange membrane by a casting method according to the present invention, the sodiumization and hydrogenation in step (5) are specifically the following steps: sodiumization of the treated membrane in step (4) with a 25wt% NaOH methanol solution and hydrogenation with a 16wt% hydrochloric acid solution, followed by washing with deionized water and drying to obtain an amphoteric perfluorosulfonic acid ion exchange membrane.

[0024] The amphoteric perfluorosulfonic acid ion exchange membrane prepared according to the method described above is used in vanadium batteries.

[0025] The present invention will be described below in conjunction with specific embodiments.

[0026] Raw materials used in the examples and comparative examples: perfluorosulfonic acid fluorine resin powder, DuPont; other raw materials, commercially available.

[0027] Example 1

[0028] (1) 100 g of perfluorosulfonic acid fluorine-type resin powder, 4 g of styrene sulfonic acid, 6 g of dimethylaminoethyl methacrylate and 1 g of p-fluorostyrene are fully mixed in a reaction kettle, 1000 g of N-methylpyrrolidone is added, the gas is evacuated and nitrogen is filled in three times, and then the reaction kettle is sealed, heated to 100° C. to completely dissolve the above raw materials, irradiated with gamma rays, the irradiation dose is 3 Mrad, cooled to room temperature, and the pressure is released to obtain a grafted mixed liquid;

[0029] (2) drying and concentrating the grafting mixed liquid described in step (1) to obtain a mother liquid;

[0030] (3) applying the mother solution of step (2) on a substrate by scraping, and obtaining a primary film by drying;

[0031] (4) subjecting the primary membrane of step (3) to gamma ray irradiation treatment at a irradiation dose of 2.5 Mrad to obtain a treated membrane;

[0032] (5) The treated membrane in step (4) was sequentially treated with a 25 wt % NaOH methanol solution and a 16 wt % hydrochloric acid solution for sodiumization, washed with deionized water, and dried to obtain an amphoteric perfluorosulfonic acid ion exchange membrane.

[0033] Example 2

[0034] (1) 100 g of perfluorosulfonic acid fluorine-type resin powder, 5 g of sodium styrene sulfonate, 9 g of methacryloyloxyethyl trimethylammonium chloride and 1.5 g of p-fluorostyrene are fully mixed in a reaction kettle, 2000 g of dimethyl sulfoxide is added, the gas is evacuated and nitrogen is filled in 3-5 times, and then the reaction kettle is sealed, heated to 105° C. to completely dissolve the above raw materials, irradiated with gamma rays, the irradiation dose is 3.5 Mrad, cooled to room temperature, and the pressure is released to obtain a grafted mixed liquid;

[0035] (2) drying and concentrating the grafting mixed liquid described in step (1) to obtain a mother liquid;

[0036] (3) applying the mother solution of step (2) on a substrate by scraping, and obtaining a primary film by drying;

[0037] (4) subjecting the primary membrane of step (3) to gamma ray irradiation treatment at a irradiation dose of 3 Mrad to obtain a treated membrane;

[0038] (5) The treated membrane in step (4) was sequentially treated with a 25 wt % NaOH methanol solution and a 16 wt % hydrochloric acid solution for sodiumization, washed with deionized water, and dried to obtain an amphoteric perfluorosulfonic acid ion exchange membrane.

[0039] Example 3

[0040] (1) 100 g of perfluorosulfonic acid fluorine resin powder, 4.5 g of 3-sulfonic acid propyl methacrylate, 7.5 g of N-isopropyl acrylamide and 1.2 g of p-fluorostyrene were fully mixed in a reaction kettle, 1500 g of N,N-dimethylformamide was added, the gas was evacuated and argon was filled in 4 times, and then the reaction kettle was sealed, heated to 102° C. to completely dissolve the above raw materials, irradiated with gamma rays, the irradiation dose was 3.2 Mrad, cooled to room temperature, and the pressure was released to obtain a grafted mixed liquid;

[0041] (2) drying and concentrating the grafting mixed liquid described in step (1) to obtain a mother liquid;

[0042] (3) applying the mother solution of step (2) on a substrate by scraping, and obtaining a primary film by drying;

[0043] (4) subjecting the primary membrane of step (3) to gamma ray irradiation treatment at a irradiation dose of 2.8 Mrad to obtain a treated membrane;

[0044] (5) The treated membrane in step (4) was sequentially treated with a 25 wt % NaOH methanol solution and a 16 wt % hydrochloric acid solution for sodiumization, washed with deionized water, and dried to obtain an amphoteric perfluorosulfonic acid ion exchange membrane.

[0045] Comparative Example 1

[0046] Except that p-fluorostyrene is not added, the other steps are the same as those in Example 3.

[0047] Performance Testing

[0048] The properties of the resins and films of the embodiments and comparative examples were tested respectively, and the specific test data are shown in Table 1 below.

[0049] Table 1

[0050] Test items Example 1 Example 2 Example 3 Comparative Example 1 Appearance Smooth surface Smooth surface Smooth surface Slightly porous surface Grafting rate / % 65.3 67.2 68.9 38.5 Thickness / um 10±0.2 10±0.2 10±0.2 10±0.8 Conductivity at 25℃ / mS / cm 106.2 106.8 108.1 101.9 <![CDATA[Vanadium ion permeability / cm -2 / cm]]> <![CDATA[0.72×10 -7 ]]> <![CDATA[0.71×10 -7 ]]> <![CDATA[0.68×10 -7 ]]> <![CDATA[1.25×10 -7 ]]>

[0051] It can be seen from the data of the embodiments and comparative examples that the present invention uses para-fluorostyrene to assist the perfluorosulfonic acid fluorine resin in the irradiation grafting modification of anions and cations, so that the grafting rate of the perfluorosulfonic acid fluorine resin is greatly improved, the branched structure further improves the viscoelasticity of the resin, and improves the film-forming property. The film product prepared by the casting method is flat and smooth, with a thinner and more uniform thickness and good dimensional stability. The conductivity retention rate of the perfluorosulfonic acid ion exchange membrane after sodium and acid treatment is high, and the vanadium ion isolation effect is significantly improved, which meets the comprehensive performance requirements for actual use.

[0052] The above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A method for preparing an amphoteric perfluorosulfonic acid ion exchange membrane by a casting method, characterized in that: The following steps are involved: (1) mixing raw materials including perfluorosulfonic acid fluorine-type resin powder, anion modifier, cationic modifier and grafting aid in a proportion in a reaction kettle, adding a solvent, removing gas and filling with inert gas, sealing, heating to 100-105° C. to completely dissolve the raw materials, irradiating with gamma rays at a dose of 3-3.5 Mrad, and cooling to room temperature to obtain a grafting mixed liquid; (2) drying and concentrating the grafting mixed liquid described in step (1) to obtain a mother liquid; (3) applying the mother solution of step (2) on a substrate by scraping, and obtaining a primary film by drying; (4) subjecting the primary membrane of step (3) to gamma ray irradiation to obtain a treated membrane; (5) subjecting the treated membrane in step (4) to sodiumization and hydrogenation to obtain an anionic and cationic perfluorosulfonic acid ion exchange membrane; The anion modifier is one or a combination of styrene sulfonic acid, sodium styrene sulfonate and 3-sulfonyl methacrylate; The cationic modifier is one or a combination of dimethylaminoethyl methacrylate, N-(4-vinylbenzyl)-N,N-dialkylamine, N-isopropylacrylamide, methacryloyloxyethyltrimethylammonium chloride and 1-allyl-3-vinylimidazole acetate; The grafting auxiliary agent is p-fluorostyrene.

2. The method for preparing amphoteric perfluorosulfonic acid ion exchange membrane by a casting method as claimed in claim 1, characterized in that: The solvent is one of N-methylpyrrolidone, dimethyl sulfoxide and N,N-dimethylformamide.

3. The method for preparing amphoteric perfluorosulfonic acid ion exchange membrane by a casting method as claimed in claim 1, characterized in that: The mass ratio of perfluorosulfonic acid fluorine resin powder, anion modifier, cationic modifier, grafting aid and solvent is 100:(4-5):(6-9):(1-1.5):(1000-2000).

4. The method for preparing amphoteric perfluorosulfonic acid ion exchange membrane by a casting method as claimed in claim 1, characterized in that: The number of times of exhausting gas and filling in inert gas in step (2) is 3-5 times; the inert gas is nitrogen or argon.

5. The method for preparing amphoteric perfluorosulfonic acid ion exchange membrane by a casting method as claimed in claim 1, characterized in that: The sodiumization and hydrogenation in step (5) are specifically to sodiumize the treated membrane in step (4) with a 25wt% NaOH methanol solution and hydrogenate it with a 16wt% hydrochloric acid solution, wash it with deionized water, and dry it to obtain an amphoteric perfluorosulfonic acid ion exchange membrane.

6. An amphoteric perfluorosulfonic acid ion exchange membrane prepared by the method according to any one of claims 1 to 5.

7. The use of the amphoteric perfluorosulfonic acid ion exchange membrane as claimed in claim 6, characterized in that: The amphoteric perfluorosulfonic acid ion exchange membrane is used in vanadium batteries.

Citation Information

Patent Citations

  • Method for preparing homogeneous-phase ion exchange membrane of all-vanadium battery by use of ray irradiation grafting method

    CN104779404A

  • Zwitter Nafion ion exchange membrane for vanadium batteries and preparation method thereof

    CN108695534A

  • Composite enhanced perfluorosulfonic acid ion exchange membrane as well as preparation method and application thereof

    CN117207626A

  • Fabrication method for the anion-exchange membranes by radiation graft cross-linking of vinylbenzyl chloride / divinylbenzene mixture and subsequent quaternarization with tertiary amines

    KR1020130130460A