A two-component thermally conductive insulating EMI shielding material and a preparation method thereof

By forming an insulating layer on the surface of metal powder and modifying it, combined with three-level particle size powder compounding, the problem of insufficient insulation and thermal conductivity of thermal shielding materials is solved, and the preparation of complex morphology materials and efficient electromagnetic Shielding effect.

CN117794212BActive Publication Date: 2024-10-15WUHAN INSTITUTES OF ADVANCED TECHNOLOGY CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311821571.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2024-10-15
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

The electrical insulation performance of existing thermally conductive shielding materials is not excellent enough, and thermally conductive powder cannot be added in large quantities, resulting in insufficient thermal conductivity and electromagnetic shielding performance. It is also difficult to prepare 3D materials and special-shaped materials with complex morphologies using existing methods.

Method used

An insulating layer is formed on the surface of the metal powder and modified with a specific silane coupling agent to obtain modified insulating metal powder. A two-component preparation method is used, combined with a three-level particle size powder compound, to form a dense thermal conductive path and insulation. layer to improve electromagnetic shielding and thermal conductivity.

Benefits of technology

It achieves efficient electromagnetic shielding performance, thermal conductivity and dielectric properties, is suitable for material preparation with complex morphology, improves the safety and service life of the material, and facilitates subsequent processing and commercial application.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of EMI electromagnetic shielding materials, and specifically to a two-component thermally conductive insulating EMI shielding material and a preparation method thereof. The two-component thermally conductive insulating EMI shielding material provided by the present invention comprises raw materials including component A and component B; in parts by weight, the component A comprises: 3.8 to 42.5 parts of double-terminal vinyl polysiloxane, 57 to 96 parts of modified insulating metal powder and 0.05 to 1 part of catalyst; in parts by weight, the component B comprises: 1.6 to 31.5 parts of double-terminal vinyl polysiloxane, 0.2 to 10 parts of double-terminal hydrogen-containing polysiloxane, 0.1 to 5.2 parts of side chain hydrogen-containing polysiloxane, 57 to 96 parts of modified insulating metal powder and 0.0005 to 0.02 parts of inhibitor. The thermally conductive insulating EMI shielding material prepared by the method of the present invention has good thermal conductivity, dielectric properties, electromagnetic shielding properties and mechanical properties, is easier to process, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of EMI electromagnetic shielding materials, and in particular to a two-component thermally conductive insulating EMI shielding material and a preparation method thereof. Background Art

[0002] As electronic devices are rapidly developing towards high integration and high frequency, electromagnetic interference (EMI) problems between electronic components have emerged. The rapid dissipation of accumulated heat and effective electromagnetic interference (EMI) shielding have attracted widespread attention. Giving thermal management materials EMI shielding properties is an effective way to overcome both heat dissipation and EMI problems. Existing metal or non-metallic conductive powders have high thermal conductivity and excellent electrical properties, and are suitable for the preparation of EMI shielding thermal management materials. By establishing a continuous conductive and thermal conductive network, excellent EMI shielding performance and high thermal conductivity can be obtained. However, existing conductive fillers will inevitably affect the electrical insulation performance, resulting in short circuits in electrical structures such as circuits.

[0003] In order to solve the above problems, researchers have tried to introduce insulating coatings on the surface of thermally conductive shielding materials, or to prepare electrically insulating EMI shielding thermal management materials by multi-layer composite with thermally conductive insulating materials. These methods can effectively improve the electrical insulation performance of EMI shielding materials and maintain their shielding performance. For example, patent application CN103722832 A discloses an insulating polymer-based electromagnetic shielding material and its preparation method. However, this method has a complex process and is only suitable for making sheets. It is not suitable for making 3D materials and special-shaped materials with complex morphology, and sheets are not conducive to subsequent processing and further utilization. In comparison, electromagnetic shielding materials with complex morphology are easier to process, which is conducive to promoting the promotion and utilization of electromagnetic shielding materials.

[0004] In addition, the existing EMI shielding materials have problems with insufficient thermal conductivity and electromagnetic shielding performance because thermal conductive powder cannot be added in large quantities. Summary of the invention

[0005] In order to solve the technical problems that the electrical insulation performance of existing thermally conductive shielding materials is not good enough, the existing insulation modification method is only suitable for modified sheets, and the thermal conductivity and electromagnetic shielding performance are not good enough, the present invention first forms an insulating layer on the surface of a metal powder to obtain an insulating metal powder, and modifies the insulating metal powder using a specific silane coupling agent to obtain a modified insulating metal powder. Finally, a two-component thermally conductive insulating EMI shielding material is prepared using the modified insulating metal powder. The thermally conductive insulating EMI shielding material contains an insulating layer, has good insulation performance, and is excellent in electromagnetic shielding effect, thermal conductivity, and dielectric properties.

[0006] The first aspect of the present invention provides a two-component thermally conductive insulating EMI shielding material, the raw materials of which include component A and component B;

[0007] By weight, the component A comprises:

[0008] 3.8-42.5 parts of double-terminal vinyl polysiloxane, 57-96 parts of modified insulating metal powder and 0.05-1 part of catalyst;

[0009] By weight, the B component comprises:

[0010] 1.6 to 31.5 parts of double-terminal vinyl polysiloxane, 0.2 to 10 parts of double-terminal hydrogen-containing polysiloxane, 0.1 to 5.2 parts of side chain hydrogen-containing polysiloxane, 57 to 96 parts of modified insulating metal powder and 0.0005 to 0.02 parts of inhibitor.

[0011] Specifically, the kinematic viscosity of the dual-terminal vinyl polysiloxane in the A component and the B component is 50 to 20,000 cps.

[0012] Specifically, the modified insulating metal powders in the A component and the B component are modified powders of metal powders and their alloys, and the metal powders are selected from at least one of Al, Mn, Mg, Cr, Ni, Nb, Mo, Cu, Fe, W, Zn, Sn, Pb, Ag, Ti, Zr, Ta, Pt and Sb;

[0013] Specifically, the surfaces of the modified insulating metal powders in the A component and the B component are both provided with insulating layers, the thickness of the insulating layers is 50 to 1000 nm, and the composition of the insulating layers is one of diamond, α-phase aluminum oxide and β-phase silicon nitride.

[0014] A second aspect of the present invention provides a method for preparing a two-component thermally conductive insulating EMI shielding material, comprising the following steps:

[0015] The A component and the B component are mixed in a mass ratio of 1:1 and reacted to obtain the two-component thermally conductive insulating EMI shielding material; the present invention adopts two components, and when the A component and the B component are mixed, they can be cured from a semi-fluid state to an elastomer;

[0016] Specifically, the preparation method of component A comprises the following steps:

[0017] Under vacuum conditions, component A is prepared using double-terminal vinyl polysiloxane, modified insulating metal powders with different particle sizes and catalysts as raw materials.

[0018] More specifically, the preparation method of component A is:

[0019] ① Mix the double-terminal vinyl polysiloxane and 0.2-5 μm modified insulating metal powder, disperse them at 1000-2000 rpm, and then stir for 10-15 minutes at a vacuum degree below -0.095 MPa;

[0020] ② Add 7-20 μm modified insulating metal powder to the mixture obtained in step ①, mix well, disperse at 800-1200 rpm, and then stir for 10-15 minutes at a vacuum degree of less than -0.095 MPa;

[0021] ③ Add 40-200 μm modified insulating metal powder to the mixture obtained in step ②, mix well, disperse at 300-1000 rpm, and then stir for 10-15 minutes at a vacuum degree of less than -0.095 MPa;

[0022] ④ heating and stirring the mixture obtained in step ③ to a temperature of 100 to 120° C., stirring at 20 to 60 rpm, and then stirring for 30 to 60 min at a vacuum degree of less than -0.095 MPa;

[0023] ⑤ Cool the mixture obtained in step ④ to room temperature, add the catalyst and mix well, and then stir for 10 to 15 minutes at a vacuum degree below -0.095 MPa to obtain the A component.

[0024] In the process of preparing component A, adding modified insulating metal powders of different particle size ranges in batches is conducive to achieving more filling of modified insulating metal powders and facilitating the dispersion of modified insulating metal powders;

[0025] More specifically, the mass ratio of the modified insulating metal powder added in step ①, step ② and step ③ is 1:2:3;

[0026] More specifically, the catalyst in step ⑤ is selected from a Custer catalyst, the component of which is a platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex, with a platinum content of 1000 to 20000 pp; too high a platinum content is not conducive to accurate addition and uniform dispersion, and too low a content will introduce too much polysiloxane;

[0027] Specifically, the preparation method of the B component is:

[0028] Under vacuum conditions, component B is prepared using double-terminal vinyl polysiloxane, modified insulating metal powders with different particle sizes, side chain hydrogen-containing polysiloxane, double-terminal hydrogen-containing polysiloxane and inhibitor as raw materials.

[0029] More specifically, the preparation method of the B component is:

[0030] (1) mixing double-terminal vinyl polysiloxane and 0.2-5 μm modified insulating metal powder, dispersing at 1000-2000 rpm, and stirring for 10-15 minutes at a vacuum degree of less than -0.095 MPa;

[0031] (2) adding 7-20 μm modified insulating metal powder to the mixture obtained in step (1) and mixing, dispersing at 800-1200 rpm, and stirring for 10-15 min at a vacuum degree of less than -0.095 MPa;

[0032] (3) adding 40-200 μm modified insulating metal powder to the mixture obtained in step (2) and mixing, dispersing at 300-1000 rpm, and then stirring for 10-15 minutes at a vacuum degree of less than -0.095 MPa;

[0033] (4) heating and stirring the mixture in step (3) to 100-120° C., stirring at 20-60 rpm, and stirring for 30-60 min at a vacuum degree of less than -0.095 MPa;

[0034] (5) The mixture in step (4) is cooled to room temperature, and the side chain hydrogen-containing polysiloxane, the double-end hydrogen-containing polysiloxane and the inhibitor are added, and stirred for 10 to 15 minutes at a vacuum degree below -0.095 MPa to obtain the B component.

[0035] More specifically, the mass ratio of the modified insulating metal powder added in step (1), step (2) and step (3) is 1:2:3;

[0036] More specifically, the kinematic viscosity of the side chain hydrogen-containing polysiloxane is 20 to 500 cps;

[0037] More specifically, the kinematic viscosity of the dual-terminal hydrogen-containing polysiloxane is 10 to 500 cps;

[0038] More specifically, the inhibitor is selected from one or more of 3-methyl-1-dodecyne-3-ol, 1-ethynyl-1-cyclohexanol, and tetramethyltetravinylcyclotetrasiloxane;

[0039] Specifically, the preparation methods of the modified insulating metal powder in the A component and the B component are:

[0040] An insulating layer is deposited on the surface of metal powder by plasma vapor phase chemical deposition to obtain insulating metal powder, and then the insulating metal powder is modified by a silane coupling agent to obtain modified insulating metal powder.

[0041] More specifically, the method of plasma chemical vapor deposition of diamond insulating layer is:

[0042] Using CH4 (purity ≥ 99.9999wt%) as the carbon source, a mixed gas of CH4 and H2 is plasmatized and continuously deposited on the surface of the metal powder at 800°C for 5 to 30 minutes; the deposition conditions are: the concentration of CH4 in the mixed gas of CH4 and H2 (purity ≥ 99.9999wt%) is 3 to 9wt%; the H2 flow rate is constant at 400sccm, and the reaction environment pressure is 0.1 to 1.0kPa.

[0043] More specifically, the method of plasma chemical vapor deposition of α-phase aluminum oxide insulating layer is:

[0044] Using trimethylaluminum (Al(CH3)3) as an aluminum source and oxygen (O2) as an oxidant source, Al(CH3)3 and O2 are plasmatized and continuously deposited on the surface of metal powder for 500 to 10,000 cycles to generate α-phase alumina on the powder surface; the thickness of the α-alumina generated in each cycle is 0.1±0.01nm, and the thickness of the α-alumina insulating layer can be controlled by adjusting the number of cycles.

[0045] More specifically, the experimental conditions for the above deposition are:

[0046] Deposition temperature: 300°C, reaction environment pressure: <10Pa;

[0047] Single cycle standard program: Al(CH3)3 injection (injection duration: 0.025 sec), purge (argon: 180 sccm, duration: 6 sec), plasma O2 exposure (20 sccm, plasma power: 300 W), purge (argon: 180 sccm, duration: 6 sec);

[0048] More specifically, the α-phase aluminum oxide insulating layer can also be prepared by aluminum alcohol hydrolysis method, and the preparation process is as follows:

[0049] An alumina precursor, an acetic acid catalyst, distilled water and isopropanol are mixed to obtain a mixed solution, and the solution is stirred at 75 to 90° C. until the system becomes transparent to obtain a γ-phase alumina colloid. A metal powder is added to the γ-phase alumina colloid, and the mixture is stirred at 1800 to 2800 rpm for 20 to 35 minutes, and then filtered and dried, and then calcined at 1200 to 1500° C. for 20 to 60 minutes to obtain the insulating metal powder. In the process, the alumina precursor used is aluminum isopropoxide, and its purity is greater than 99%. The mass ratio of distilled water to isopropanol in the mixed solution is 3.5 to 4.5:1, the content of the alumina precursor is 14.28 to 30.6 wt%, and the weight of the acetic acid catalyst accounts for 0.6 to 1.2 wt%; the mass ratio of the γ-phase alumina colloid to the metal powder is 2.5 to 3.5:1.

[0050] More specifically, the method for preparing insulating metal powder containing β-phase silicon nitride insulating layer by plasma chemical vapor deposition is as follows:

[0051] NH3 and SiH4 are used as precursors, NH3 and SiH4 are plasmatized, the gas flow rate of NH3 is controlled to be 100-350sccm and the gas flow rate of SiH4 is controlled to be 100sccm, the reaction environment pressure is 10-30Pa, the temperature is 80-100°C, and the deposition time is 5-80min, α-phase silicon nitride can be generated on the surface of the powder, and the powder is calcined at 1500-1700°C for 20-60min to obtain an insulating metal powder containing a β-phase silicon nitride insulating layer;

[0052] More specifically, the silane coupling agent is a silane coupling agent with an alkane main chain, and the silane coupling agent with an alkane main chain does not contain amino groups and epoxy groups;

[0053] More specifically, the specific method of modifying the insulating metal powder with a silane coupling agent is:

[0054] Add acetic acid to pure water to adjust the pH value to 3-4, then add ethanol and stir at 100-300rpm for 2-5min, add silane coupling agent and stir at 100-300rpm for 2-5min, then add insulating metal powder and stir at 150-400rpm, heat to 60-75°C and continue stirring for 1-2h, filter to remove the aqueous solution and heat to 110-120°C, stir at 200-600rpm for 0.5-1h in vacuum, constant temperature, and finally cool to room temperature to obtain the modified insulating metal powder; the vacuum degree of the vacuum is <-0.1MPa;

[0055] More specifically, the mass ratio of the insulating metal powder, the silane coupling agent, the pure water and the ethanol is 95-99: 0.25-1.8: 0.3-1.5: 0.4-4;

[0056] More specifically, its general structural formula is: CH3-(CH2)n-Si-(OCH3)3, the selection of n has a great influence on the performance of the insulating metal powder, and n is preferably an integer of 5 to 17;

[0057] The -(OCH3)3 structure carried by the silane coupling agent can react with the hydroxyl group on the surface of the powder after hydrolysis, and then can graft a carbon chain on the surface of the insulating metal powder to achieve the hydrophobic and lipophilic properties of the surface of the insulating metal powder, and can improve the wettability of the insulating metal powder in the polysiloxane system, reduce the viscosity of the mixture formed when the modified insulating metal powder is mixed with the polysiloxane in the system, and can achieve a higher metal powder filling amount. At the same time, it can reduce the microscopic interface thermal resistance of the metal powder and the polysiloxane, thereby improving the thermal conductivity, and can also greatly improve the tensile strength of the cured material, so that it has higher mechanical properties; the other end of the silane coupling agent is a carbon chain, does not contain amino and epoxy groups, and can ensure that the catalyst of the two-component addition-type silicone in the present invention has catalytic activity.

[0058] The technical effects brought by the method of the present invention are as follows:

[0059] 1. The present invention uses metal powder coated with a high thermal conductivity insulating layer on the surface as filler, supplemented with three-grade particle size powder for compounding, thereby achieving dense filling, constructing a large number of thermal conductive paths, and making the material have good thermal conductivity; in addition, the dense insulating layer coated on the surface of the metal powder can effectively block the conductive connection between the powders, avoiding the formation of an overall large-area conductive network, improving the electrical insulation performance of the material, and improving its safety and service life;

[0060] 2. When the incident electromagnetic wave radiates to the surface of the shielding material during use, most of the electromagnetic wave is reflected due to the impedance mismatch between the external free space and the shielding material. The residual electromagnetic wave that penetrates the surface of the shielding material is reflected multiple times between the metal powders and attenuated until it is fully absorbed and finally dissipated in the form of heat. When the alternating EM encounters the metal powder inside the shielding material of the present invention, it will also cause the combined effects of hysteresis loss, eddy current loss, relaxation loss, current loss, polarization loss, etc., resulting in higher losses. Finally, the thermally conductive insulating EMI shielding material prepared by the present invention can achieve good electromagnetic wave shielding in the frequency band of 10Hz to 45GHz, and has excellent electromagnetic shielding performance.

[0061] 3. The present invention solves the problem that the existing EMI shielding materials cannot be dispensed into special shapes and can only be made into sheets, resulting in greatly limited application scenarios. It is more convenient for subsequent processing and also realizes the integration of the thermal conductivity, insulation and shielding functions of metal powders, which is beneficial to the promotion and commercial application of thermal conductive insulating EMI shielding materials and has good application prospects. DETAILED DESCRIPTION

[0062] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0063] In addition, it should be noted that the "parts" of raw materials added in the examples are parts by weight unless otherwise specified.

[0064] Example 1

[0065] 1. Preparation of modified insulating metal powder:

[0066] Using CH4 (purity ≥ 99.9999wt%) as a carbon source, CH4 and H2 are plasmatized and continuously deposited on the surface of Al metal powder at 800°C for 15 minutes to obtain an insulating metal powder containing a diamond insulating layer; the deposition conditions are: a mixed gas of CH4 and H2 (purity ≥ 99.9999wt%), the concentration of CH4 in the mixed gas is 6wt%, the H2 flow rate is constant at 400sccm, and the reaction environment pressure is 0.5kPa.

[0067] Then add acetic acid to 0.9 parts of pure water to adjust the pH value to 3.5, then add 2 parts of ethanol and stir at 200 rpm for 3.5 minutes, add 1 part of silane coupling agent (CH3-(CH2) 11 -Si-(OCH3)3) was stirred at 200 rpm for 3.5 min, then 97 parts of the above-mentioned insulating metal powder was added and heated to 67°C, and then stirred at 280 rpm for 1.5 h, the aqueous solution was filtered to remove, and then heated to 115°C, and then stirred at a vacuum (vacuum degree -0.3 MPa), constant temperature and 400 rpm for 0.8 h, and finally cooled to room temperature and sieved to obtain 3μm, 14μm and 120μm modified insulating metal powders.

[0068] 2. Preparation of the A component:

[0069] ① Mix 23.2 parts of double-terminated vinyl polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-Vi303) and 12.7 parts of 3μm modified insulating metal powder, stir at 40rpm, disperse at 1500rpm, and then stir at a vacuum degree of -0.1MPa for 12min;

[0070] ② Add 25.3 parts of 14 μm modified insulating metal powder to the mixture obtained in step ①, stir at 40 rpm, disperse at 1000 rpm, and then stir for 12 minutes at a vacuum degree of less than -0.1 MPa;

[0071] ③ Add 38.0 parts of 120 μm modified insulating metal powder to the mixture obtained in step ②, stir at 40 rpm, disperse at 650 rpm, and then stir at a vacuum degree of -0.2 MPa for 12 minutes;

[0072] ④ Heat and stir the mixture obtained in step ③ to a temperature of 110°C, stir at 40 rpm, and then stir for 45 min at a vacuum degree of -0.1 MPa;

[0073] ⑤ Cool the mixture obtained in step ④ to room temperature, add 0.07 parts of platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Dongguan Daochen Chemical Electronic Materials Co., Ltd., model DC-pt10000), stir at 50 rpm, and then stir for 13 minutes at a vacuum degree of -0.2 MPa to obtain the A component.

[0074] 3. Preparation of component B:

[0075] (1) 16.6 parts of double-terminated vinyl polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-Vi303) and 12.7 parts of 3 μm modified insulating metal powder were mixed, stirred at 40 rpm, dispersed at 1500 rpm, and then stirred for 12 min at a vacuum degree of -0.2 MPa;

[0076] (2) adding 25.3 parts of 14 μm modified insulating metal powder to the mixture obtained in step (1), stirring at 40 rpm, dispersing at 1000 rpm, and stirring for 12 min at a vacuum degree of -0.2 MPa;

[0077] (3) adding 38 parts of 120 μm modified insulating metal powder to the mixture obtained in step (2), stirring at 40 rpm, dispersing at 650 rpm, and stirring for 12 min at a vacuum degree of -0.2 MPa;

[0078] (4) heating and stirring the mixture in step (3) to 110° C., stirring at 40 rpm, and then stirring for 45 min under a vacuum degree of −0.2 MPa;

[0079] (5) The mixture in step (4) was cooled to room temperature, 2.6 parts of side chain hydrogen-containing polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-H3), 5 parts of double-end hydrogen-containing polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-DH04) and 0.01 parts of 3-methyl-1-dodecyne-3-ol were added, and the mixture was stirred for 12 minutes under a vacuum degree of -0.2 MPa to obtain the B component.

[0080] 4. Preparation of two-component thermally conductive insulating EMI shielding materials:

[0081] The two-component thermally conductive insulating EMI shielding material is obtained by mixing component A and component B in a mass ratio of 1:1 and reacting them.

[0082] Example 2

[0083] 1. Preparation of modified insulating metal powder:

[0084] Using CH4 (purity ≥ 99.9999wt%) as a carbon source, CH4 and H2 are plasmatized and continuously deposited on the surface of Mn metal powder at 800°C for 5 minutes to obtain an insulating metal powder containing a diamond insulating layer; the deposition conditions are: a mixed gas of CH4 and H2 (purity ≥ 99.9999wt%), the concentration of CH4 in the mixed gas is 3wt%, the H2 flow rate is constant at 400sccm, and the reaction environment pressure is 0.1kPa.

[0085] Acetic acid was added to 0.3 parts of pure water to adjust the pH value to 3, and then 0.4 parts of ethanol was added and stirred at 100 rpm for 2 minutes, 0.25 parts of silane coupling agent (CH3-(CH2)5-Si-(OCH3)3) was added and stirred at 100 rpm for 2 minutes, and then 95 parts of insulating metal powder were added and stirred at 150 rpm. After heating to 60°C, stirring was continued for 1 hour, the aqueous solution was filtered to remove, and then heated to 110°C, and stirred at a constant temperature and 200 rpm for 0.5 hours. Finally, it was cooled to room temperature and sieved to obtain 0.2μm, 7μm and 120μm modified insulating metal powders.

[0086] 2. Preparation of the A component:

[0087] ① Mix 3.8 parts of double-terminated vinyl polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-Vi395) and 9.5 parts of 0.2 μm modified insulating metal powder, stir at 20 rpm, disperse at 1000 rpm, and then stir for 10 min at a vacuum degree of -0.15 MPa;

[0088] ② Add 19 parts of 7 μm modified insulating metal powder to the mixture obtained in step ①, stir at 20 rpm, disperse at 800 rpm, and then stir for 10 minutes at a vacuum degree of -0.095 MPa;

[0089] ③ Add 28.5 parts of 120 μm modified insulating metal powder to the mixture obtained in step ②, stir at 20 rpm, disperse at 300 rpm, and then stir for 10 minutes at a vacuum degree of -0.2 MPa;

[0090] ④ Heat and stir the mixture obtained in step ③ to a temperature of 100°C, stir at 20 rpm, and then stir for 30 min at a vacuum degree of -0.2 MPa;

[0091] ⑤ Cool the mixture obtained in step ④ to room temperature, add 0.05 parts of platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Dongguan Daochen Chemical Electronic Materials Co., Ltd., Model DC-pt1000), stir at 40 rpm, and then stir for 10 minutes at a vacuum degree of -0.2 MPa to obtain the A component.

[0092] 3. Preparation of component B:

[0093] (1) 1.6 parts of double-terminated vinyl polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-Vi395) and 9.5 parts of 3 μm modified insulating metal powder were mixed, stirred at 20 rpm, dispersed at 1000 rpm, and then stirred for 10 min at a vacuum degree of -0.15 MPa;

[0094] (2) adding 19 parts of 7 μm modified insulating metal powder to the mixture obtained in step (1), stirring at 20 rpm, dispersing at 800 rpm, and stirring for 10 min at a vacuum degree of -0.15 MPa;

[0095] (3) Add 38.5 parts of 120 μm modified insulating metal powder to the mixture obtained in step (2), stir at 20 rpm, disperse at 300 rpm, and then stir for 10 min at a vacuum degree of less than -0.15 MPa;

[0096] (4) heating and stirring the mixture in step (3) to 100° C., stirring at 20 rpm, and then stirring for 30 min at a vacuum degree of less than -0.15 MPa;

[0097] (5) The mixture in step (4) was cooled to room temperature, 0.1 parts of side chain hydrogen-containing polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-H95), 0.2 parts of double-end hydrogen-containing polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-H45) and 0.0005 parts of 1-ethynyl-1-cyclohexanol were added, and the mixture was stirred at a vacuum degree of -0.15 MPa for 10 minutes to obtain the B component.

[0098] 4. Preparation of two-component thermally conductive insulating EMI shielding materials:

[0099] The two-component thermally conductive insulating EMI shielding material is obtained by mixing component A and component B in a mass ratio of 1:1 and reacting them.

[0100] Example 3

[0101] 1. Preparation of modified insulating metal powder:

[0102] Using CH4 (purity ≥99.9999wt%) as a carbon source, CH4 and H2 are plasmatized and continuously deposited on the surface of Ti metal powder at 800°C for 30 minutes to obtain an insulating metal powder containing a diamond insulating layer; the deposition conditions are: a mixed gas of CH4 and H2 (purity ≥99.9999wt%), the concentration of CH4 in the mixed gas is 9wt%, the H2 flow rate is constant at 400sccm, and the reaction environment pressure is 1.0kPa.

[0103] Add acetic acid to 1.5 parts of pure water to adjust the pH to 4, then add 4 parts of ethanol and stir at 300 rpm for 5 minutes, then add 1.8 parts of silane coupling agent (CH3-(CH2) 17 -Si-(OCH3)3) was stirred at 300 rpm for 5 min, then 99 parts of insulating metal powder was added and stirred at 400 rpm, and the mixture was heated to 75°C and stirred for 2 h. The aqueous solution was filtered out and heated to 120°C. The mixture was stirred at a constant temperature and 600 rpm for 1 h in a vacuum (vacuum degree -0.2 MPa). Finally, the mixture was cooled to room temperature and sieved to obtain 5 μm, 20 μm and 200 μm modified insulating metal powders.

[0104] 2. Preparation of the A component:

[0105] ① Mix 42.5 parts of double-terminated vinyl polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-Vi302) and 16 parts of 5μm modified insulating metal powder, stir at 60rpm, disperse at 2000rpm, and then stir for 15min at a vacuum degree of -0.2MPa;

[0106] ② Add 32 parts of 20 μm modified insulating metal powder to the mixture obtained in step ①, stir at 60 rpm, disperse at 1200 rpm, and then stir for 15 minutes at a vacuum degree of -0.15 MPa;

[0107] ③ Add 48 parts of 200 μm modified insulating metal powder to the mixture obtained in step ②, stir at 60 rpm, disperse at 1000 rpm, and then stir for 15 minutes at a vacuum degree of -0.2 MPa;

[0108] ④ Heat and stir the mixture obtained in step ③ to a temperature of 120°C, stir at 60 rpm, and then stir for 60 min at a vacuum degree of -0.2 MPa;

[0109] ⑤ Cool the mixture obtained in step ④ to room temperature, add 1 part of platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Dongguan Daochen Chemical Electronic Materials Co., Ltd., model DC-pt20000), stir at 60 rpm, and then stir for 15 minutes at a vacuum degree of -0.2 MPa to obtain the A component.

[0110] 3. Preparation of component B:

[0111] (1) 31.5 parts of double-terminated vinyl polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-Vi302) and 16 parts of 5 μm modified insulating metal powder were mixed, stirred at 60 rpm, dispersed at 2000 rpm, and then stirred for 15 min at a vacuum degree of -0.2 MPa;

[0112] (2) adding 32 parts of 20 μm modified insulating metal powder to the mixture obtained in step (1), stirring at 60 rpm, dispersing at 1200 rpm, and stirring for 15 min at a vacuum degree of -0.2 MPa;

[0113] (3) adding 48 parts of 200 μm modified insulating metal powder to the mixture obtained in step (2), stirring at 60 rpm, dispersing at 1000 rpm, and stirring for 15 min at a vacuum degree of -0.2 MPa;

[0114] (4) heating and stirring the mixture in step (3) to 120° C., stirring at 60 rpm, and then stirring for 60 min under a vacuum degree of −0.2 MPa;

[0115] (5) The mixture in step (4) was cooled to room temperature, 5.2 parts of side chain hydrogen-containing polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-H138), 10 parts of double-end hydrogen-containing polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-DH02) and 0.02 parts of tetramethyltetravinylcyclotetrasiloxane were added, and the mixture was stirred for 15 minutes under a vacuum degree of -0.2 MPa to obtain the B component.

[0116] 4. Preparation of two-component thermally conductive insulating EMI shielding materials:

[0117] The two-component thermally conductive insulating EMI shielding material is obtained by mixing component A and component B in a mass ratio of 1:1 and reacting them.

[0118] Example 4

[0119] 1. Preparation of modified insulating metal powder:

[0120] Using trimethylaluminum (Al(CH3)3) as the aluminum source and oxygen (O2) as the oxidant source, Al(CH3)3 and O2 are plasmatized and continuously deposited on the surface of the metal powder for 5000 cycles, and α-phase aluminum oxide can be generated on the surface of the powder; the experimental conditions for deposition are: deposition temperature: 300°C, reaction environment pressure: 9Pa; single cycle standard procedure: Al(CH3)3 injection (injection duration: 0.025 seconds), purge (argon: 180sccm, duration: 6 seconds), plasma O2 exposure (20sccm, plasma power: 300W), purge (argon: 180sccm, duration: 6 seconds);

[0121] Add acetic acid to 0.9 parts of pure water to adjust the pH to 3.5, then add 2 parts of ethanol and stir at 200 rpm for 3.5 minutes, then add 1 part of silane coupling agent (CH3-(CH2) 11 -Si-(OCH3)3) was stirred at 200 rpm for 3.5 min, then 97 parts of insulating metal powder was added and stirred at 280 rpm, and the mixture was heated to 67°C and stirred for 1.5 h. The aqueous solution was filtered to remove the aqueous solution, and then heated to 115°C, kept constant temperature under vacuum (vacuum degree -0.3 MPa) and stirred at 400 rpm for 0.8 h. Finally, it was cooled to room temperature and sieved to obtain 0.2 μm, 7 μm and 120 μm modified insulating metal powders.

[0122] 2. Preparation of the A component:

[0123] The preparation process of component A in this embodiment is the same as that in embodiment 2.

[0124] 3. Preparation of component B:

[0125] The preparation process of component B in this embodiment is the same as that in Example 2.

[0126] 4. Preparation of two-component thermally conductive insulating EMI shielding materials:

[0127] The preparation process of the two-component thermally conductive insulating EMI shielding material is the same as that of Example 1.

[0128] Example 5

[0129] 1. Preparation of modified insulating metal powder:

[0130] NH3 and SiH4 are used as precursors, NH3 and SiH4 are plasmatized, the gas flow of NH3 is controlled to be 200 sccm and the gas flow of SiH4 is controlled to be 100 sccm, the reaction environment pressure is 20 Pa, the temperature is maintained at 90°C, and α-phase silicon nitride is continuously deposited on the surface of Zn metal powder for 40 minutes, and then calcined at 1600°C for 40 minutes to obtain insulating metal powder containing β-phase silicon nitride insulating layer;

[0131] Acetic acid was added to 0.3 parts of pure water to adjust the pH value to 3, and then 0.4 parts of ethanol was added and stirred at 100 rpm for 2 minutes, 0.25 parts of silane coupling agent (CH3-(CH2)5-Si-(OCH3)3) was added and stirred at 100 rpm for 2 minutes, and then 95 parts of insulating metal powder were added and stirred at 150 rpm. After heating to 60°C, stirring was continued for 1 hour, the aqueous solution was filtered to remove, and then heated to 110°C. It was stirred at a constant temperature and 200 rpm for 0.5 hours in a vacuum (vacuum degree -0.2MPa), and finally cooled to room temperature and sieved to obtain 5μm, 20μm and 200μm modified insulating metal powders.

[0132] 2. Preparation of the A component:

[0133] The preparation process of component A in this embodiment is the same as that in embodiment 3.

[0134] 3. Preparation of component B:

[0135] The preparation process of component B in this embodiment is the same as that in embodiment 3.

[0136] 4. Preparation of two-component thermally conductive insulating EMI shielding materials:

[0137] The preparation of the two-component thermally conductive insulating EMI shielding material is the same as in Example 1.

[0138] Example 6

[0139] 1. Preparation of modified insulating metal powder:

[0140] 22 parts of aluminum isopropoxide (purity> 99%), 0.9 parts of acetic acid catalyst and 61.7 parts of distilled water are mixed with 15.4 parts of isopropanol for hydrolysis, and stirred at 82°C until the system is transparent to obtain a γ-phase alumina colloid, 25 parts of Fe metal powder are added to the γ-phase alumina colloid, stirred at 2300 rpm for 20 to 35 minutes, then filtered and dried, and then calcined at 1350°C for 30 minutes to obtain an insulating metal powder of an α-phase alumina insulating layer;

[0141] Add acetic acid to 1.5 parts of pure water to adjust the pH to 4, then add 4 parts of ethanol and stir at 300 rpm for 5 minutes, then add 1.8 parts of silane coupling agent (CH3-(CH2) 17 -Si-(OCH3)3) was stirred at 300 rpm for 5 min, then 99 parts of insulating metal powder was added and stirred at 400 rpm, and the mixture was heated to 75°C and stirred for 2 h. The aqueous solution was filtered to remove the solution, and then heated to 120°C, and stirred at a constant temperature and 600 rpm for 1 h in a vacuum (vacuum degree -0.2 MPa). Finally, the mixture was cooled to room temperature and sieved to obtain 3 μm, 14 μm and 120 μm modified insulating metal powders.

[0142] 2. Preparation of the A component:

[0143] The preparation process of component A in this embodiment is the same as that in embodiment 1.

[0144] 3. Preparation of component B:

[0145] The preparation process of component B in this embodiment is the same as that in embodiment 1.

[0146] 4. Preparation of two-component thermally conductive insulating EMI shielding materials:

[0147] The preparation of the two-component thermally conductive insulating EMI shielding material is the same as in Example 1.

[0148] Comparative Example 1

[0149] 1. Preparation of modified insulating metal powder:

[0150] Add acetic acid to 0.9 parts of pure water to adjust the pH to 3.5, then add 2 parts of ethanol and stir at 200 rpm for 3.5 minutes, then add 1 part of silane coupling agent (CH3-(CH2) 11 -Si-(OCH3)3) was stirred at 200 rpm for 3.5 min, then 97 parts of Al metal powder was added and stirred at 280 rpm, and the mixture was heated to 67°C and stirred for 1.5 h. The aqueous solution was filtered out and heated to 115°C. The mixture was stirred at a constant temperature and 400 rpm for 0.8 h in a vacuum (vacuum degree -0.3 MPa). Finally, the mixture was cooled to room temperature and sieved to obtain 3 μm, 14 μm and 120 μm modified insulating metal powders.

[0151] 2. Preparation of the A component:

[0152] The preparation process of component A in this embodiment is the same as that in embodiment 1.

[0153] 3. Preparation of component B:

[0154] The preparation process of component B in this embodiment is the same as that in embodiment 1.

[0155] 4. Preparation of two-component thermally conductive insulating EMI shielding materials:

[0156] The preparation of the two-component thermally conductive insulating EMI shielding material is the same as in Example 1.

[0157] Comparative Example 2

[0158] 1. Preparation of modified insulating metal powder:

[0159] CH4 (purity ≥ 99.9999wt%) was used as the carbon source, and the concentration of CH4 in the mixed gas of CH4 and H2 (purity ≥ 99.9999wt%) was 6wt%. CH4 and H2 were plasmatized, the H2 flow rate was constant at 400sccm, the reaction environment pressure was 0.5kPa, and deposition was continued on the surface of Al metal powder at 800°C for 15 minutes to obtain insulating metal powder containing a diamond insulating layer.

[0160] Acetic acid was added to 0.9 parts of pure water to adjust the pH value to 3.5, and then 2 parts of ethanol were added and stirred at 200 rpm for 3.5 minutes, 1 part of silane coupling agent (CH3-(CH2)4-Si-(OCH3)3) was added and stirred at 200 rpm for 3.5 minutes, and then 97 parts of insulating metal powder were added and stirred at 280 rpm. At the same time, the mixture was heated to 67°C and stirred for 1.5 hours. The aqueous solution was filtered out and heated to 115°C. The mixture was stirred at a constant temperature and 400 rpm for 0.8 hours. Finally, the mixture was cooled to room temperature and sieved to obtain 3μm, 14μm and 120μm modified insulating metal powders.

[0161] 2. Preparation of the A component:

[0162] The preparation process of component A in this embodiment is the same as that in embodiment 1.

[0163] 3. Preparation of component B:

[0164] The preparation process of component B in this embodiment is the same as that in embodiment 1.

[0165] 4. Preparation of two-component thermally conductive insulating EMI shielding materials:

[0166] The preparation of the two-component thermally conductive insulating EMI shielding material is the same as in Example 1.

[0167] Comparative Example 3

[0168] 1. Preparation of modified insulating metal powder:

[0169] CH4 (purity ≥ 99.9999wt%) was used as the carbon source, and the concentration of CH4 in the mixed gas of CH4 and H2 (purity ≥ 99.9999wt%) was 6wt%. CH4 and H2 were plasmatized, the H2 flow rate was constant at 400sccm, the reaction environment pressure was 0.5kPa, and deposition was continued on the surface of Al metal powder at 800°C for 15 minutes to obtain insulating metal powder containing a diamond insulating layer.

[0170] Add acetic acid to 0.9 parts of pure water to adjust the pH to 3.5, then add 2 parts of ethanol and stir at 200 rpm for 3.5 minutes, then add 1 part of silane coupling agent (CH3-(CH2) 18 -Si-(OCH3)3) was stirred at 200 rpm for 3.5 min, then 97 parts of insulating metal powder was added and stirred at 280 rpm, and the mixture was heated to 67°C and stirred for 1.5 h. The aqueous solution was filtered out and heated to 115°C. The mixture was stirred at a constant temperature and 400 rpm for 0.8 h in a vacuum (vacuum degree -0.3 MPa). Finally, the mixture was cooled to room temperature and sieved to obtain 3 μm, 14 μm and 120 μm modified insulating metal powders.

[0171] 2. Preparation of the A component:

[0172] The preparation process of component A in this embodiment is the same as that in embodiment 1.

[0173] 3. Preparation of component B:

[0174] The preparation process of component B in this embodiment is the same as that in embodiment 1.

[0175] 4. Preparation of two-component thermally conductive insulating EMI shielding materials:

[0176] The preparation of the two-component thermally conductive insulating EMI shielding material is the same as in Example 1.

[0177] Comparative Example 4

[0178] 1. Preparation of modified insulating metal powder:

[0179] The preparation of the modified insulating metal powder is the same as that in Example 1.

[0180] 2. Preparation of the A component:

[0181] ① Mix 23.2 parts of double-terminated vinyl polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-Vi303) and 76 parts of modified insulating metal powder (the mass ratio of 3 μm, 14 μm and 120 μm is 1:2:3), stir at 400 rpm, disperse at 1500 rpm, and then stir at a vacuum degree of -0.1 MPa for 40 min;

[0182] ② The mixture obtained in step ① was heated and stirred to a temperature of 110° C., stirred at 40 rpm, and then stirred at a vacuum degree of -0.1 MPa for 45 min;

[0183] ③ Cool the mixture obtained in step ② to room temperature, add 0.07 parts of platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Dongguan Daochen Chemical Electronic Materials Co., Ltd., model DC-pt10000), stir at 50 rpm, and then stir for 13 minutes at a vacuum degree of -0.2 MPa to obtain the A component.

[0184] 3. Preparation of component B:

[0185] (1) 16.6 parts of double-terminated vinyl polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-Vi303) and 76 parts of modified insulating metal powder (3 μm) were mixed, stirred at 400 rpm, dispersed at 1500 rpm, and then stirred at a vacuum degree of -0.2 MPa for 40 min;

[0186] (2) heating and stirring the mixture in step (1) to 110° C., stirring at 40 rpm, and then stirring for 45 min under a vacuum degree of −0.2 MPa;

[0187] (3) The mixture in step (2) was cooled to room temperature, 2.6 parts of side chain hydrogen-containing polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-H3), 5 parts of double-end hydrogen-containing polysiloxane (Ningbo Runhe New Materials Technology Co., Ltd., brand RH-DH04) and 0.01 parts of 3-methyl-1-dodecyne-3-ol were added, and the mixture was stirred for 12 minutes under a vacuum degree of -0.2 MPa to obtain the B component.

[0188] 4. Preparation of two-component thermally conductive insulating EMI shielding materials:

[0189] The preparation of the two-component thermally conductive insulating EMI shielding material is the same as in Example 1.

[0190] Performance Testing

[0191] The performance of the two-component thermally conductive insulating EMI shielding materials prepared in the examples and comparative examples was tested, and the test results are shown in Table 1.

[0192] Test items Shielding effectiveness (dB) Dielectric strength (KV / mm) Thermal conductivity (W / m·K) Tensile strength(Mpa) Example 1 55 2.5 6.8 2.1 Example 2 56 1.6 6.1 1.6 Example 3 38 3.3 3.2 3.2 Example 4 41 1.9 2.8 1.7 Example 5 45 2.3 3.1 1.8 Example 6 46 2.6 2.7 2.6 Comparative Example 1 54 0.001 5.9 1.4 Comparative Example 2 43 1.2 3.6 1.1 Comparative Example 3 54 2.4 2.1 1.2 Comparative Example 4 54 0.6 2.3 1.6

[0193] The embodiment of the present invention adopts the method of the present invention to prepare a two-component thermally conductive insulating EMI shielding material, and the obtained two-component thermally conductive insulating EMI shielding material has good shielding energy efficiency, dielectric strength, thermal conductivity and mechanical properties; Comparative Example 1 has poor dielectric properties because the metal powder is not coated with an insulating layer; Comparative Example 2 has a silane coupling agent n less than 5, and the -(OCH3)3 on it will be more easily hydrolyzed, resulting in self-polymerization before it can be grafted to the powder surface, resulting in poor powder modification effect, affecting the shielding performance, dielectric strength, thermal conductivity and mechanical properties; Comparative Example 3 has a silane coupling agent n greater than 17, the corresponding carbon chain segment is longer, the molecular weight is larger, and the thickness of the coating grafted on the powder surface is larger, which will affect the powder contact and thereby reduce the thermal conductivity; Comparative Example 4 adds the modified insulating metal powder at one time when preparing component A and component B, which makes it difficult for the powder to be evenly dispersed in the polysiloxane, thereby resulting in poor dielectric strength and thermal conductivity.

Claims

1. A method for preparing a two-component thermally conductive insulating EMI shielding material, It is characterized in that The following steps are involved: The component A and the component B are mixed in a mass ratio of 1:1 and reacted to obtain the two-component thermally conductive insulating EMI shielding material; The preparation method of the A component is: Under vacuum conditions, component A is prepared using double-terminal vinyl polysiloxane, modified insulating metal powders of different particle sizes and catalysts as raw materials; The preparation method of the B component comprises the following steps: Under vacuum conditions, component B is prepared using double-terminal vinyl polysiloxane, modified insulating metal powders of different particle sizes, side chain hydrogen-containing polysiloxane, double-terminal hydrogen-containing polysiloxane and inhibitor as raw materials; The preparation methods of the modified insulating metal powders are: Depositing an insulating layer on the surface of the metal powder by plasma vapor phase chemical deposition to obtain an insulating metal powder, and then modifying the insulating metal powder with a silane coupling agent to obtain the modified insulating metal powder; The method for modifying insulating metal powder with a silane coupling agent is: Acetic acid is added to pure water to adjust the pH value to 3-4, then ethanol is added and stirred at 100-300 rpm for 2-5 minutes, a silane coupling agent is added and stirred at 100-300 rpm for 2-5 minutes, then insulating metal powder is added and stirred at 150-400 rpm, and the mixture is heated to 60-75° C. and stirred continuously for 1-2 hours. After filtering to remove the aqueous solution, the mixture is heated to 110-120° C., stirred at a constant temperature in a vacuum state and at 200-600 rpm for 0.5-1 hour, and finally cooled to room temperature to obtain the modified insulating metal powder.

2. The method for preparing the two-component thermally conductive insulating EMI shielding material according to claim 1, It is characterized in that The silane coupling agent is an alkane main chain silane coupling agent, and its general structural formula is CH3-(CH2)n-Si-(OCH3)3, wherein n is an integer of 5 to 17.

3. The method for preparing the two-component thermally conductive insulating EMI shielding material according to claim 1, It is characterized in that The mass ratio of the insulating metal powder, the silane coupling agent, pure water and ethanol is 95-99: 0.25-1.8: 0.3-1.5: 0.4-4.

4. A two-component thermally conductive insulating EMI shielding material prepared according to the method according to any one of claims 1 to 3.