A high-strength, high-stability, high-flame-retardant polyurethane foam material free of ODS substances and its preparation method and application

By using composite flame retardant and specific ratio polyurethane materials, the problems of flammability and construction difficulty of polyurethane rigid foam for spray-coated cold storage are solved, and polyurethane foam with high strength, high stability and low GWP value are achieved , reduces costs and improves security.

CN117801202BActive Publication Date: 2024-11-05HENAN DUORUN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311846802.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-05
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

The existing polyurethane hard foam for spray-type cold storage is flammable and requires explosion-proof equipment, resulting in high cost; it is difficult to construct, poor strength and dimensional stability, and has a low service life.

Method used

Using composite flame retardant and specific ratio polyurethane foaming materials, including isocyanate, composite flame retardant polyester polyol, composite polyether polyol, composite silicone oil, catalyst and foaming agent, high strength and high stability are prepared through reaction and mixing. Polyurethane foaming material with high flame retardancy and no ODS substances.

Benefits of technology

It realizes high flame retardancy of polyurethane foamed materials, reduces the investment cost of spray-coated cold storage, improves liquidity and strength, enhances dimensional stability, significantly reduces GWP value, and improves production and application safety guarantees.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the field of polyurethane technology. It discloses a high-strength, high-stability, high-flame-retardant polyurethane foam material free of ODS substances, its preparation method, and its application. The polyurethane foam material comprises component A and component B; the mass ratio of component A to component B is 1-1.2:1; component A includes isocyanate; component B comprises the following components in parts by mass: 70-90 parts of composite flame-retardant polyester polyol, 10-25 parts of composite polyether polyol, 1-5 parts of composite silicone oil, 5-7 parts of catalyst, 30-45 parts of composite flame retardant, 5-10 parts of foaming agent, and 2-5 parts of water. This invention obtains a polyurethane foam material with non-flammable properties through the compounding of composite flame retardants; the polyurethane foam material obtained by this invention has a lower thermal conductivity, better flowability, better strength and dimensional stability, and a lower GWP value; compared with other foaming systems, it has higher production and application safety assurance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane, and in particular to a polyurethane foam material with high strength, high stability, high flame retardancy and no ODS substance, and a preparation method and application thereof. Background Art

[0002] Polyurethane rigid foam is a high molecular polymer made of isocyanate and polyether as the main raw materials, mixed by special equipment under the action of various additives such as foaming agent, catalyst, flame retardant, etc., and foamed on site by high-pressure spraying. There are two types of polyurethane foam: soft foam and hard foam. Soft foam is an open-cell structure, and hard foam is a closed-cell structure; soft foam is divided into two types: crusting and non-skinning. Cold storage spraying, also known as polyurethane insulation spraying. Cold storage spraying is a spraying technology. The closed-cell rate of polyurethane rigid foam is ≥95%, the water absorption rate is ≤1%, and it has good energy-saving and heat-insulating effects. Polyurethane rigid foam is a high-density closed-cell foam compound with a thermal conductivity of ≤0.022W / mk (the average temperature of the hot and cold plates is 12.5℃), and it has good energy-saving effects. Therefore, polyurethane rigid foam has been widely developed in spray-type cold storage.

[0003] However, the existing spray-coated polyurethane rigid foam for cold storage does not meet the requirements of environmental protection, and it is difficult to achieve a high flame retardant effect. In particular, the controlled substance 141B specified in the Montreal Protocol is also facing elimination as a foaming agent, and the selectivity of alternative substances is relatively narrow, resulting in a significant increase in costs. In addition, the existing spray-coated polyurethane rigid foam for cold storage has poor tolerance and is difficult to construct; the feed density is large and the dimensional stability is poor, and the maintenance cost is high. Therefore, the field urgently needs to develop a polyurethane foam material that has the characteristics of being completely free of CFC substances, and has a lower thermal conductivity, better cost advantages, strength and dimensional stability, and a lower GWP value. Summary of the invention

[0004] The purpose of the present invention is to provide a polyurethane foam material with high strength, high stability, high flame retardancy and no ODS substances, and a preparation method and application thereof, so as to solve the problem that the existing polyurethane rigid foam for spray-type cold storage is flammable, explosion-proof equipment needs to be installed to ensure the safety of the cold storage, resulting in a greatly increased cost; it also solves the problem that the existing polyurethane rigid foam for spray-type cold storage has poor fluidity and is difficult to construct; it has poor strength and dimensional stability and a short service life.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] The invention provides a polyurethane foam material with high strength, high stability, high flame retardancy and no ODS substances. The polyurethane foam material comprises a component A and a component B; the mass ratio of the component A to the component B is 1-1.2:1; the component A comprises isocyanate; the component B comprises the following components in mass fractions: 70-90 parts of a composite flame-retardant polyester polyol, 10-25 parts of a composite polyether polyol, 1-5 parts of a composite silicone oil, 5-7 parts of a catalyst, 30-45 parts of a composite flame retardant, 5-10 parts of a foaming agent and 2-5 parts of water.

[0007] Preferably, the composite flame-retardant polyester polyol comprises polyethylene adipate, polybutylene adipate and poly-ε-caprolactone diol; the mass ratio of polyethylene adipate, polybutylene adipate and poly-ε-caprolactone diol is 1:1~2:1~1.5; the composite polyether polyol comprises polypropylene glycol and polytetrahydrofuran diol; the mass ratio of polypropylene glycol and polytetrahydrofuran diol is 1~3:1.

[0008] Preferably, the composite silicone oil comprises amino silicone oil and hydroxy silicone oil, and the mass ratio of amino silicone oil to hydroxy silicone oil is 2~4:1; the catalyst comprises 1,8-diazabicycloundec-7-ene and / or 1,5-diazabicyclo(4,3,0)non-5-ene; and the foaming agent is LBA foaming agent.

[0009] Preferably, the composite flame retardant includes purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol, tetrabutyl titanate and tris(1-chloro-2-propyl) phosphate.

[0010] Preferably, the mass ratio of purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate is 3000-4000:1000-2000:5000-6000:500-1000:0.1-1; the amount of tri(1-chloro-2-propyl) phosphate is 5-15% of the total mass of purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate.

[0011] The present invention also provides a method for preparing the high-strength, high-stability, high-flame-retardant polyurethane foam material that does not contain ODS substances, comprising the following steps:

[0012] (1) Purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate are mixed and reacted to obtain a reactive flame retardant, and the reactive flame retardant and tri(1-chloro-2-propyl) phosphate are mixed to obtain a composite flame retardant;

[0013] (2) mixing a composite flame-retardant polyester polyol, a composite polyether polyol, a composite silicone oil, a catalyst, a composite flame retardant, a foaming agent and water to obtain a component B;

[0014] (3) Taking isocyanate as component A; mixing component A and component B and foaming them to obtain a polyurethane foam material.

[0015] Preferably, in step (1), the reaction temperature is 160-230° C., the reaction time is 1-5 h, and the reactive flame retardant and tri(1-chloro-2-propyl) phosphate are mixed for 1-10 min.

[0016] Preferably, in step (2), the mixing is carried out under stirring conditions, the stirring speed of the mixing is 3000-4000 r / min, the mixing time is 10-30 min, and the mixing temperature is 20-30° C.

[0017] Preferably, in step (3), the mixing and foaming is carried out under stirring conditions, the stirring speed of the mixing and foaming is 2000-3000 r / min, the mixing and foaming time is 10-20 min, and the mixing and foaming temperature is 20-30°C.

[0018] The present invention also provides the use of the polyurethane foam material with high strength, high stability, high flame retardancy and no ODS substance in a spray-type cold storage.

[0019] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention prepares a polyurethane foam material with non-flammable characteristics by compounding and using a composite flame retardant, which can avoid the investment in explosion-proof equipment and significantly reduce the investment cost of a spray-type cold storage; the polyurethane foam material obtained by the present invention has lower thermal conductivity, better fluidity, better strength and dimensional stability, and lower GWP value; and has higher production and application safety guarantees compared to other foaming systems. DETAILED DESCRIPTION

[0021] The invention provides a polyurethane foam material with high strength, high stability, high flame retardancy and no ODS substances. The polyurethane foam material comprises a component A and a component B; the mass ratio of the component A to the component B is 1-1.2:1; the component A comprises isocyanate; the component B comprises the following components in mass fractions: 70-90 parts of a composite flame-retardant polyester polyol, 10-25 parts of a composite polyether polyol, 1-5 parts of a composite silicone oil, 5-7 parts of a catalyst, 30-45 parts of a composite flame retardant, 5-10 parts of a foaming agent and 2-5 parts of water.

[0022] In the present invention, the mass ratio of component A to component B is preferably 1.05 to 1.15:1, and more preferably 1.1:1.

[0023] In the A component of the present invention, the isocyanate includes isophorone diisocyanate or polyphenyl polymethylene polyisocyanate.

[0024] In component B of the present invention, the amount of composite flame-retardant polyester polyol is preferably 75-85 parts, more preferably 78-80 parts; the amount of composite polyether polyol is preferably 15-20 parts, more preferably 16-18 parts; the amount of composite silicone oil is preferably 2-4 parts, more preferably 3-3.5 parts; the amount of catalyst is preferably 5.5-6.5 parts, more preferably 6 parts; the amount of composite flame retardant is preferably 35-40 parts, more preferably 38-39 parts; the amount of foaming agent is preferably 6-9 parts, more preferably 7-8 parts; the amount of water is preferably 3-4 parts, more preferably 3.5 parts.

[0025] In the present invention, the composite flame-retardant polyester polyol comprises polyethylene adipate, polybutylene adipate and poly-ε-caprolactone diol; the mass ratio of polyethylene adipate, polybutylene adipate and poly-ε-caprolactone diol is preferably 1:1~2:1~1.5, and more preferably 1:1.2~1.5:1.2~1.4; the composite polyether polyol comprises polypropylene glycol and polytetrahydrofuran diol; the mass ratio of polypropylene glycol and polytetrahydrofuran diol is preferably 1~3:1, and more preferably 1.5~2:1.

[0026] In the present invention, the composite silicone oil comprises amino silicone oil and hydroxy silicone oil, and the mass ratio of amino silicone oil to hydroxy silicone oil is preferably 2-4:1, and further preferably 2.5-3:1; the catalyst comprises 1,8-diazabicycloundec-7-ene and / or 1,5-diazabicyclo(4,3,0)non-5-ene; and the foaming agent is LBA foaming agent.

[0027] In the present invention, the composite flame retardant comprises purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol, tetrabutyl titanate and tris(1-chloro-2-propyl) phosphate.

[0028] In the present invention, the mass ratio of purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate is preferably 3000-4000: 1000-2000: 5000-6000: 500-1000: 0.1-1, and more preferably 3200-3800: 1300-1800: 5100-5500: 600-800: 0.5-0.8; the amount of tri(1-chloro-2-propyl) phosphate is preferably 5-15% of the total mass of purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate, and more preferably 8-10% of the total mass of purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate.

[0029] The present invention also provides a method for preparing the high-strength, high-stability, high-flame-retardant polyurethane foam material that does not contain ODS substances, comprising the following steps:

[0030] (1) Purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate are mixed and reacted to obtain a reactive flame retardant, and the reactive flame retardant and tri(1-chloro-2-propyl) phosphate are mixed to obtain a composite flame retardant;

[0031] (2) mixing a composite flame-retardant polyester polyol, a composite polyether polyol, a composite silicone oil, a catalyst, a composite flame retardant, a foaming agent and water to obtain a component B;

[0032] (3) Taking isocyanate as component A; mixing component A and component B and foaming them to obtain a polyurethane foam material.

[0033] In step (1) of the present invention, the reaction temperature is preferably 160-230° C., more preferably 180-200° C.; the reaction time is preferably 1-5 h, more preferably 2-4 h; the mixing time of the reactive flame retardant and tris(1-chloro-2-propyl) phosphate is preferably 1-10 min, more preferably 5-8 min.

[0034] In step (2) of the present invention, mixing is carried out under stirring conditions, and the stirring speed of the mixing is preferably 3000-4000 r / min, more preferably 3200-3500 r / min; the mixing time is preferably 10-30 min, more preferably 20-25 min; the mixing temperature is preferably 20-30° C., more preferably 22-28° C.

[0035] In step (3) of the present invention, the mixing and foaming is carried out under stirring conditions. The stirring speed of the mixing and foaming is preferably 2000-3000 r / min, and more preferably 2500-2800 r / min. The mixing and foaming time is preferably 10-20 min, and more preferably 12-15 min. The mixing and foaming temperature is preferably 20-30°C, and more preferably 22-28°C.

[0036] The present invention also provides the use of the polyurethane foam material with high strength, high stability, high flame retardancy and no ODS substance in a spray-type cold storage.

[0037] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention. Example 1

[0038] Preparation of composite flame retardant:

[0039] The raw materials and their amounts are: 300 parts of purified terephthalic acid, 100 parts of isopropyl alcohol, 550 parts of diethylene glycol, 80 parts of neopentyl glycol, 0.1 parts of tetrabutyl titanate and 123.612 parts of tris(1-chloro-2-propyl) phosphate;

[0040] The preparation process is:

[0041] The above-mentioned mass fractions of purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate are reacted at 180° C. for 3 hours to obtain a reactive flame retardant; the above-mentioned mass fractions of tri(1-chloro-2-propyl) phosphate are added to the reactive flame retardant and mixed at room temperature for 8 minutes to obtain a composite flame retardant. Example 2

[0042] Preparation of composite flame retardant:

[0043] The raw materials used and their amounts are: 350 parts of purified terephthalic acid, 120 parts of isopropyl alcohol, 500 parts of diethylene glycol, 70 parts of neopentyl glycol, 0.1 parts of tetrabutyl titanate and 124.812 parts of tris(1-chloro-2-propyl) phosphate;

[0044] The preparation process is:

[0045] The above-mentioned mass fractions of purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate are reacted at 190° C. for 4 hours to obtain a reactive flame retardant; the above-mentioned mass fractions of tri(1-chloro-2-propyl) phosphate are added to the reactive flame retardant and mixed at room temperature for 10 minutes to obtain a composite flame retardant. Example 3

[0046] Preparation of composite flame retardant:

[0047] The raw materials and their amounts are: 400 parts of purified terephthalic acid, 180 parts of isopropyl alcohol, 520 parts of diethylene glycol, 80 parts of neopentyl glycol, 0.1 parts of tetrabutyl titanate and 118.01 parts of tris(1-chloro-2-propyl) phosphate;

[0048] The preparation process is:

[0049] The above-mentioned mass fractions of purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate are reacted at 220° C. for 5 hours to obtain a reactive flame retardant; the above-mentioned mass fractions of tri(1-chloro-2-propyl) phosphate are added to the reactive flame retardant and mixed at room temperature for 7 minutes to obtain a composite flame retardant. Example 4

[0050] Preparation of polyurethane foam material:

[0051] The raw materials used and their amounts are: 20 parts of polyethylene adipate, 40 parts of polybutylene adipate, 20 parts of poly-ε-caprolactone diol, 9 parts of polypropylene glycol, 9 parts of polytetrahydrofuran diol, 2.5 parts of amino silicone oil, 1 part of hydroxy silicone oil, 5.5 parts of 1,5-diazabicyclo (4,3,0) non-5-ene, 40 parts of the composite flame retardant obtained in Example 1, 8 parts of LBA foaming agent, 4 parts of water, and 166.95 parts of polyphenyl polymethylene polyisocyanate;

[0052] The preparation process is:

[0053] The above-mentioned mass fractions of polyethylene adipate, polybutylene adipate, poly-ε-caprolactone diol, polypropylene glycol, polytetrahydrofuran diol, amino silicone oil, hydroxy silicone oil, 1,5-diazabicyclo (4,3,0) non-5-ene, the composite flame retardant obtained in Example 1, LBA foaming agent and water are stirred and mixed at a speed of 3200 r / min at room temperature for 25 minutes to obtain component B; component B and the above-mentioned mass fractions of polyphenyl polymethylene polyisocyanate are mixed and foamed at a stirring speed of 2500 r / min at room temperature for 15 minutes to obtain a polyurethane foam material.

[0054] After testing, the compressive strength of the polyurethane foam material obtained in this embodiment is 168MPa, and the core density is 43kg / m 3 The milky time of the polyurethane foam material is 3s, the gel time is 8s, and the surface drying time is 11s. Example 5

[0055] Preparation of polyurethane foam material:

[0056] The raw materials used and their amounts are: 20 parts of polyethylene adipate, 30 parts of polybutylene adipate, 30 parts of poly-ε-caprolactone diol, 12 parts of polypropylene glycol, 6 parts of polytetrahydrofuran diol, 2.5 parts of amino silicone oil, 1 part of hydroxy silicone oil, 5.5 parts of 1,8-diazabicycloundec-7-ene, 40 parts of the composite flame retardant obtained in Example 2, 8 parts of LBA foaming agent, 4 parts of water, and 166.95 parts of polyphenyl polymethylene polyisocyanate;

[0057] The preparation process is:

[0058] The above-mentioned mass fractions of polyethylene adipate, polybutylene adipate, poly-ε-caprolactone diol, polypropylene glycol, polytetrahydrofuran diol, amino silicone oil, hydroxy silicone oil, 1,8-diazabicycloundec-7-ene, the composite flame retardant obtained in Example 2, LBA foaming agent and water are stirred and mixed at a speed of 3500 r / min at room temperature for 20 minutes to obtain component B; component B and the above-mentioned mass fractions of polyphenyl polymethylene polyisocyanate are mixed and foamed at a stirring speed of 2800 r / min at room temperature for 12 minutes to obtain a polyurethane foam material.

[0059] After testing, the compressive strength of the polyurethane foam material obtained in this embodiment is 167MPa, and the core density is 44kg / m 3 The milky time of the polyurethane foam material is 3s, the gel time is 9s, and the surface drying time is 12s. Example 6

[0060] Preparation of polyurethane foam material:

[0061] The raw materials used and their amounts are: 20 parts of polyethylene adipate, 30 parts of polybutylene adipate, 30 parts of poly-ε-caprolactone diol, 15 parts of polypropylene glycol, 5 parts of polytetrahydrofuran diol, 2.5 parts of amino silicone oil, 1 part of hydroxy silicone oil, 5.5 parts of 1,8-diazabicycloundec-7-ene, 40 parts of the composite flame retardant obtained in Example 3, 8 parts of LBA foaming agent, 4 parts of water, and 185.15 parts of isophorone diisocyanate;

[0062] The preparation process is:

[0063] The above-mentioned mass fractions of polyethylene adipate, polybutylene adipate, poly-ε-caprolactone diol, polypropylene glycol, polytetrahydrofuran diol, amino silicone oil, hydroxy silicone oil, 1,8-diazabicycloundec-7-ene, the composite flame retardant obtained in Example 3, LBA foaming agent and water were stirred and mixed at a speed of 3800 r / min at room temperature for 20 minutes to obtain component B; component B and the above-mentioned mass fractions of isophorone diisocyanate were mixed and foamed at a stirring speed of 3000 r / min at room temperature for 12 minutes to obtain a polyurethane foam material.

[0064] After testing, the compressive strength of the polyurethane foam material obtained in this embodiment is 168MPa, and the core density is 45kg / m 3 The milky time of the polyurethane foam material is 4s, the gel time is 10s, and the surface drying time is 11s.

[0065] Comparative Example 1

[0066] The composite flame retardant in Example 4 was replaced by diethyl ethyl phosphate, and the rest was the same as in Example 4.

[0067] The compressive strength of the obtained polyurethane foam material is 143MPa and the core density is 28kg / m 3 The milky time of the polyurethane foam material is 2s, the gel time is 20s, and the surface drying time is 30s.

[0068] Comparative Example 2

[0069] The difference from Example 4 is that the addition of polyethylene adipate and polybutylene adipate is omitted, and the rest is the same as Example 4.

[0070] The compressive strength of the obtained polyurethane foam material is 152MPa and the core density is 30kg / m 3 The milky time of the polyurethane foam material is 2s, the gel time is 22s, and the surface drying time is 28s.

[0071] Comparative Example 3

[0072] The difference with embodiment 4 is: omit the interpolation of polytetrahydrofuran diol, other is with embodiment 4.

[0073] After testing, the compressive strength of the obtained polyurethane foam material is 141MPa and the core density is 26kg / m 3 The milky time of the polyurethane foam material is 2s, the gel time is 25s, and the surface drying time is 32s.

[0074] The properties of the polyurethane foam materials obtained in Examples 4 to 6 and Comparative Examples 1 to 3 were tested according to the following standards, and the results are shown in Table 1.

[0075] Testing standards: The density of the foamed material is measured according to GB / T 6343-2009; the thermal conductivity of the foamed material is measured according to GB / T 10295-2008; the bonding strength, oxygen index, dimensional stability and combustion performance of the foamed material are measured according to JC936-2004.

[0076]

[0077] It can be seen from Examples 4 to 6, Comparative Examples 1 to 3 and Table 1 that the polyurethane foam material obtained by the present invention has lower thermal conductivity, better fluidity, better strength and dimensional stability, and lower GWP value, and the flame retardant level of the obtained polyurethane foam material is significantly improved.

[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A high-strength, high-stability, high-flame-retardant polyurethane foam material that does not contain ODS substances, characterized in that: The polyurethane foam material comprises component A and component B; the mass ratio of component A to component B is 1-1.2:1; component A comprises isocyanate; component B comprises the following components in mass parts: 70-90 parts of composite flame-retardant polyester polyol, 10-25 parts of composite polyether polyol, 1-5 parts of composite silicone oil, 5-7 parts of catalyst, 30-45 parts of composite flame retardant, 5-10 parts of foaming agent and 2-5 parts of water; The composite flame-retardant polyester polyol comprises polyethylene adipate, polybutylene adipate and poly-ε-caprolactone diol; the mass ratio of polyethylene adipate, polybutylene adipate and poly-ε-caprolactone diol is 1:1-2:1-1.5; the composite polyether polyol comprises polypropylene glycol and polytetrahydrofuran diol; the mass ratio of polypropylene glycol and polytetrahydrofuran diol is 1-3:1; The composite silicone oil comprises amino silicone oil and hydroxy silicone oil, and the mass ratio of amino silicone oil to hydroxy silicone oil is 2-4:1; the catalyst comprises 1,8-diazabicycloundec-7-ene and / or 1,5-diazabicyclo(4,3,0)non-5-ene; the foaming agent is LBA foaming agent; The composite flame retardant comprises purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol, tetrabutyl titanate and tris(1-chloro-2-propyl) phosphate; The method for preparing the high-strength, high-stability, high-flame-retardant polyurethane foam material containing no ODS substances comprises the following steps: (1) Purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate are mixed and reacted to obtain a reactive flame retardant, and the reactive flame retardant and tri(1-chloro-2-propyl) phosphate are mixed to obtain a composite flame retardant; (2) mixing a composite flame-retardant polyester polyol, a composite polyether polyol, a composite silicone oil, a catalyst, a composite flame retardant, a foaming agent and water to obtain a component B; (3) Taking isocyanate as component A; mixing component A and component B and foaming them to obtain a polyurethane foam material.

2. The high-strength, high-stability, high-flame-retardant polyurethane foam material containing no ODS substances according to claim 1, characterized in that: The mass ratio of purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate is 3000-4000: 1000-2000: 5000-6000: 500-1000: 0.1-1; The dosage of tri(1-chloro-2-propyl) phosphate is 5-15% of the total weight of purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate.

3. The method for preparing the high-strength, high-stability, high-flame-retardant polyurethane foam material containing no ODS substances according to claim 1 or 2, characterized in that: The steps include: (1) Purified terephthalic acid, isopropyl alcohol, diethylene glycol, neopentyl glycol and tetrabutyl titanate are mixed and reacted to obtain a reactive flame retardant, and the reactive flame retardant and tri(1-chloro-2-propyl) phosphate are mixed to obtain a composite flame retardant; (2) mixing a composite flame-retardant polyester polyol, a composite polyether polyol, a composite silicone oil, a catalyst, a composite flame retardant, a foaming agent and water to obtain a component B; (3) Taking isocyanate as component A; mixing component A and component B and foaming them to obtain a polyurethane foam material.

4. The method for preparing the high-strength, high-stability, high-flame-retardant polyurethane foam material containing no ODS substances according to claim 3, characterized in that: In the step (1), the reaction temperature is 160-230° C., and the reaction time is 1-5 hours; the reaction flame retardant and tri(1-chloro-2-propyl) phosphate are mixed for 1-10 minutes.

5. The method for preparing the high-strength, high-stability, high-flame-retardant polyurethane foam material containing no ODS substances according to claim 4, characterized in that: In the step (2), the mixing is carried out under stirring conditions, the stirring speed of the mixing is 3000-4000 r / min, the mixing time is 10-30 min, and the mixing temperature is 20-30° C.

6. The method for preparing the high-strength, high-stability, high-flame-retardant polyurethane foam material containing no ODS substances according to claim 4 or 5, characterized in that: In the step (3), the mixing and foaming is carried out under stirring conditions, the stirring speed of the mixing and foaming is 2000-3000 r / min, the mixing and foaming time is 10-20 min, and the mixing and foaming temperature is 20-30° C.

7. Use of the high-strength, high-stability, high-flame-retardant, ODS-free polyurethane foam material according to claim 1 or 2 in a spray-type cold storage.