A cross-linked polyimide insulating dielectric film and its preparation method and application

By using the polycondensation and crosslinking treatment technology under vacuum conditions in polyimide dielectric materials, a crosslinked polyimide insulating dielectric film with high insulation characteristics was prepared, and the intrinsic insulation characteristics of polyimide dielectric materials were solved. The poor problem significantly improves the energy storage density and charge and discharge efficiency under high temperature and high fields.

CN117801274BActive Publication Date: 2024-11-15HARBIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311778999.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2024-11-15
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

The inherent insulation characteristics of existing polyimide dielectric materials are poor, resulting in a decrease in breakdown field strength and service life, and the introduction of high volume fraction inorganic fillers leads to an increase in energy loss.

Method used

The fluorinated polyamic acid glue solution was prepared by using fluorinated diamine and fluorinated dianhydride polycondensation under vacuum conditions, and a crosslinking agent was added for micro-crosslinking. Then, the wet film was prepared by coating method and microwave-assisted thermal imidation was performed. The crosslinked polyimide insulating dielectric film was formed.

Benefits of technology

Under high temperature and high field conditions, the cross-linked fluorinated polyimide dielectric film has higher energy storage density and higher charge and discharge efficiency, and the stability of the chain segment structure is enhanced. The three-dimensional cross-linked network structure of the material improves the molecules The interstitial force extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117801274B_ABST
    Figure CN117801274B_ABST
Patent Text Reader

Abstract

The present invention discloses a cross-linked polyimide insulating dielectric film and a preparation method and application thereof, belonging to the technical field of polyimide-based modified composite materials and their preparation. The present invention solves the technical problem that the existing polyimide dielectric materials have poor intrinsic insulation properties. The present invention firstly uses fluorinated dianhydride and fluorinated diamine to react to generate fluorinated polyamic acid, then adds cage-type octaaminophenylsilsesquioxane as a cross-linking agent, utilizes the amino group in the cross-linking agent to react with the carboxyl group in the fluorinated polyamic acid to achieve mutual cross-linking, and then obtains a micro-cross-linked fluorinated polyimide dielectric film after microwave-assisted imidization. The obtained film has a higher energy storage density while maintaining a higher charge and discharge efficiency under high temperature and high field conditions. Specifically, at 150°C, the energy storage density of the composite dielectric at 580MV / m is 4.18J / cm 3 , and the energy storage efficiency remains above 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a cross-linked polyimide insulating dielectric film and a preparation method and application thereof, belonging to the technical field of polyimide-based modified composite materials and preparation thereof. Background Art

[0002] With the rapid development of information, power electronics and chemical industries, especially the development of smart grids, aerospace, hybrid vehicles and high-end military weapons, the demand for insulating materials has been greatly stimulated, and there is an urgent need to develop electrical materials with high insulation properties. Polyimide (PI), as a type of high-performance polymer, is an organic polymer material with relatively excellent comprehensive performance due to its excellent dielectric properties, thermal stability and solvent resistance. It is known as the "gold of engineering plastics" in the polymer industry and is widely used in motors, electronics, aerospace and other fields, especially for slot insulation, winding insulation and dielectric buffer layers of motors, all of which require polyimide to have excellent electrical insulation properties. Therefore, the development of polyimide thin flexible insulating media with high insulation properties and its process methods has become one of the important research directions of the power equipment manufacturing industry.

[0003] In order to solve the problem of low breakdown field strength of polyimide, the existing technology adopts the method of inorganic phase doping modification or surface modification of fillers to prepare composite dielectric materials with high insulation properties. However, the introduction of high volume fraction inorganic fillers and poor compatibility cause carrier traps to be generated inside the material, resulting in increased energy loss, and reducing the breakdown field strength and service life of the material. Therefore, in the current technology, starting from the molecular structure of polyimide, optimizing its insulation properties from the intrinsic structure has become an important research hotspot.

[0004] Therefore, for polyimide dielectric materials, how to design polyimide flexible dielectric materials that intrinsically have excellent insulation properties has become an existing technical problem. Summary of the invention

[0005] In order to solve the technical problem that the existing polyimide dielectric materials have poor intrinsic insulation properties, the present invention provides a polyimide-based composite dielectric film and a preparation method thereof and application in electrical insulation, especially application in polyimide intrinsic modification technology.

[0006] The technical solution of the present invention:

[0007] One of the purposes of the present invention is to provide a method for preparing a cross-linked polyimide insulating medium, the method comprising the following steps:

[0008] (1) preparing a fluorinated polyamic acid glue solution by polycondensation of a fluorinated diamine and a fluorinated dianhydride under vacuum conditions;

[0009] (2) adding a crosslinking agent to the fluorinated polyamic acid glue solution under vacuum conditions and stirring to obtain a slightly crosslinked fluorinated polyamic acid glue solution;

[0010] (3) A coating method is used to prepare a wet film using a slightly cross-linked fluorinated polyamic acid glue solution, and the wet film is subjected to microwave-assisted thermal imidization treatment to obtain a cross-linked polyimide insulating dielectric film.

[0011] It is further defined that the specific operation process of (1) is: adding the fluorinated diamine into the organic solvent, stirring to completely dissolve it, and then adding the fluorinated dianhydride, and performing polycondensation reaction under vacuum conditions to obtain the fluorinated polyamic acid glue solution.

[0012] In further limitation, the fluorine-containing diamine in (1) is an aromatic trifluoromethyldiamine monomer, and the fluorine-containing dianhydride is an aromatic hexafluorodianhydride monomer.

[0013] In a further embodiment, the fluorine-containing diamine is 2,2'-bis(trifluoromethyl)diaminobiphenyl, and the fluorine-containing dianhydride is 4,4'-(hexafluoroisopropylene)diphthalic anhydride.

[0014] It is further defined that the molar ratio of the fluorine-containing diamine to the fluorine-containing dianhydride in (1) is (1-1.08):(1.02-1.2).

[0015] It is further defined that the mass fractions of the fluorinated diamine and the fluorinated dianhydride in the polycondensation system are both 12% to 35%.

[0016] It is further defined that the organic solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, and tetrahydrofuran mixed in any proportion.

[0017] It is further defined that the polycondensation reaction temperature in (1) is -10 to 40°C and the reaction time is 2 to 24 hours.

[0018] It is further defined that the polycondensation temperature in (1) is -5 to 10°C and the time is 2 to 24 hours.

[0019] It is further defined that the vacuum conditions in (1) and (2) are achieved by a step vacuum method, wherein the vacuum gradient interval of each step vacuum is 1 to 5 Pa, the vacuum rate is 1 to 2 Pa / min, and the constant vacuum time of each step is 30 to 180 min.

[0020] It is further defined that the crosslinking agent in (2) is any one of cage-type octaaminophenylsilsesquioxane and triaminopyrimidine, and the content of amino groups added to the crosslinking agent is 0.1% to 10% of the total molar amount of amino groups in the fluorinated diamine.

[0021] It is further defined that the specific operation process in (3) is: pouring the slightly cross-linked cross-linked fluorinated polyamide acid glue solution on the clean glass base surface, coating it on the glass substrate by scraping, spin coating or drop coating to form a wet film, and subjecting it to microwave-assisted thermal imidization treatment, and naturally cooling it to room temperature to obtain a cross-linked polyimide insulating dielectric film.

[0022] It is further defined that the coating speed of the scraper coating is 10 to 25 cm / min and the time is 10 to 60 s.

[0023] It is further defined that the coating speed of the scraper coating is 15 to 20 cm / min and the time is 10 to 60 s.

[0024] It is further defined that the coating speed of the scraper coating is 15 to 20 cm / min and the time is 20 to 40 s.

[0025] It is further defined that the microwave-assisted thermal imidization treatment conditions in (3) are: microwave power is 1000W to 5000W, thermal imidization is gradient heating, each temperature gradient interval of the gradient heating is 20 to 100°C, the heating rate is 3 to 15°C / min, and the constant temperature time of each section is 30 to 720min.

[0026] The second object of the present invention is to provide a cross-linked polyimide insulating dielectric film obtained by the above preparation method, wherein the thickness of the film is 3 to 20 μm.

[0027] The third object of the present invention is to provide an application of the cross-linked polyimide insulating dielectric film, specifically, as a high-field insulator for the preparation of electrical insulating devices.

[0028] Beneficial effects:

[0029] The present invention firstly uses fluorinated dianhydride and fluorinated diamine to react to generate fluorinated polyamic acid (F-PAA), then adds cage-type octaaminophenylsilsesquioxane and triaminopyrimidine as a crosslinking agent, utilizes the amino group in the crosslinking agent to react with the carboxyl group in F-PAA to achieve mutual crosslinking, and then obtains a micro-crosslinked fluorinated polyimide dielectric film after microwave-assisted imidization. Compared with the prior art, the modified polyimide-based composite dielectric prepared by the present invention has the following advantages:

[0030] (1) The three-dimensional cross-linked network structure of the polyimide-based composite dielectric prepared by the invention has strong stability under high temperature and high field. The segment structure is not easy to break under strong impact, which enhances the intermolecular force between the chains. This makes the cross-linked fluorinated polyimide dielectric film have higher energy storage density and maintain high charge and discharge efficiency under high temperature and high field conditions. Specifically, at 150°C, the energy storage density of the OAPS-0.5 / F-PI composite dielectric at 580MV / m is 4.18J / cm3 , an increase of 40% over F-PI dielectric materials, and the energy storage efficiency remains above 90%.

[0031] (2) In addition, the present invention has the advantages of simple preparation process and required equipment, safety and reliability, low cost, and is more conducive to its wide application in electrical insulation devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The chemical structure formula of the cross-linking agent cage-type octaaminophenylsilsesquioxane;

[0033] Figure 2 is the chemical structural formula of the cross-linking agent triaminopyrimidine;

[0034] Figure 3 XRD patterns of the polyimide-based insulating media prepared in Examples 1 to 3 and Comparative Example 1;

[0035] Figure 4 XRD patterns of the polyimide-based insulating media prepared in Comparative Example 1 and Comparative Example 2;

[0036] Figure 5 It is a comparative curve diagram of infrared spectra of the polyimide-based insulating medium prepared in Examples 1 to 3 and Comparative Example 1;

[0037] Figure 6 It is a comparative curve diagram of infrared spectra of the polyimide-based insulating medium prepared in Comparative Example 1 and Comparative Example 2;

[0038] Figure 7 The variation trend of the discharge energy density of the polyimide-based insulating medium prepared in Example 2, Comparative Example 1 and Comparative Example 2 at 150° C. with the electric field;

[0039] Figure 8 The charge and discharge efficiency of the polyimide-based insulating medium prepared in Example 2, Comparative Example and Comparative Example 21 at 150°C varies with the electric field. DETAILED DESCRIPTION

[0040] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0041] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0042] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0043] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.

[0044] Example 1

[0045] Step 1: In a 250 ml round-bottom flask, 2.1135 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl was dissolved in 25.0 ml of N,N-dimethylacetamide. Under vacuum, 2.9926 g of 4,4'-(hexafluoroisopropylene)diphthalic anhydride was added to the solution in batches at a uniform interval, and the solution was stirred under gradient vacuum. The gradient vacuum was carried out in six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, and the vacuum rate was 1 ° C / min. Each vacuum process was maintained for 120 min. After stirring for 12 hours, a fluorinated polyamic acid glue solution with a solid content of about 15% was obtained;

[0046] Step 2: Add 0.0035 g of cage-type octaaminophenylsilsesquioxane to the fluorinated polyamic acid glue solution, continue to use gradient vacuum stirring, the gradient vacuum is divided into six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, the vacuum rate is 1 ° C / min, each vacuum process is maintained for 240 min, and after stirring for 24 hours, a slightly cross-linked fluorinated polyamic acid glue solution with a solid content of about 15% is obtained;

[0047] Step three, placing the micro-cross-linked fluorinated polyamide acid glue solution in a vacuum oven for degassing treatment, and then coating it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s, and then subjected to microwave-assisted gradient heating thermal imidization treatment with a microwave power of 1000 w. The gradient heating is carried out in seven steps, 60°C → 80°C → 150°C → 200°C → 250°C → 300°C → 350°C, with a heating rate of 5°C / min, and the insulation time of each insulation process is 60 min. Finally, a micro-cross-linked fluorinated polyimide film with a thickness of 12 μm is prepared, which is recorded as OAPS-0.3 / F-PI.

[0048] Example 2

[0049] Step 1: In a 250 ml round-bottom flask, 2.1135 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl was dissolved in 25.0 ml of N,N-dimethylacetamide. Under vacuum, 2.9926 g of 4,4'-(hexafluoroisopropylene)diphthalic anhydride was added to the solution in batches at a uniform interval, and the solution was stirred under gradient vacuum. The gradient vacuum was carried out in six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, and the vacuum rate was 1 ° C / min. Each vacuum process was maintained for 120 min. After stirring for 12 hours, a fluorinated polyamic acid glue solution with a solid content of about 15% was obtained;

[0050] Step 2: Add 0.0058 g of cage-type octaaminophenylsilsesquioxane to the fluorinated polyamic acid glue solution, continue to use gradient vacuum stirring, the gradient vacuum is divided into six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, the vacuum rate is 1 ° C / min, each vacuum process is maintained for 240 min, and after stirring for 24 hours, a slightly cross-linked fluorinated polyamic acid glue solution with a solid content of about 15% is obtained;

[0051] Step three, placing the micro-cross-linked fluorinated polyamide acid glue solution in a vacuum oven for degassing treatment, and then coating it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s, and then subjected to microwave-assisted gradient heating thermal imidization treatment with a microwave power of 1000 w. The gradient heating is carried out in seven steps, 60°C → 80°C → 150°C → 200°C → 250°C → 300°C → 350°C, with a heating rate of 5°C / min, and the insulation time of each insulation process is 60 min. Finally, a micro-cross-linked fluorinated polyimide film with a thickness of 12 μm is prepared, which is recorded as OAPS-0.5 / F-PI.

[0052] Example 3

[0053] Step 1: In a 250 ml round-bottom flask, 2.1135 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl was dissolved in 25.0 ml of N,N-dimethylacetamide. Under vacuum, 2.9926 g of 4,4'-(hexafluoroisopropylene)diphthalic anhydride was added to the solution in batches at a uniform interval, and the solution was stirred under gradient vacuum. The gradient vacuum was carried out in six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, and the vacuum rate was 1 ° C / min. Each vacuum process was maintained for 120 min. After stirring for 12 hours, a fluorinated polyamic acid glue solution with a solid content of about 15% was obtained;

[0054] Step 2: Add 0.0115 g of cage-type octaaminophenylsilsesquioxane to the fluorinated polyamic acid glue solution, continue to use gradient vacuum stirring, the gradient vacuum is divided into six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, the vacuum rate is 1 ° C / min, each vacuum process is maintained for 240 min, and after stirring for 24 hours, a slightly cross-linked fluorinated polyamic acid glue solution with a solid content of about 15% is obtained;

[0055] Step three, placing the micro-cross-linked fluorinated polyamide acid glue solution in a vacuum oven for degassing treatment, and then coating it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s, and then subjected to microwave-assisted gradient heating thermal imidization treatment with a microwave power of 1000 w. The gradient heating is carried out in seven steps, 60°C → 80°C → 150°C → 200°C → 250°C → 300°C → 350°C, with a heating rate of 5°C / min, and the insulation time of each insulation process is 60 min. Finally, a micro-cross-linked fluorinated polyimide film with a thickness of 12 μm is prepared, which is recorded as OAPS-1 / F-PI.

[0056] Comparative Example 1

[0057] Step 1: In a 250 ml round-bottom flask, 2.1135 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl was dissolved in 25.0 ml of N,N-dimethylacetamide. Under vacuum, 2.9926 g of 4,4'-(hexafluoroisopropylene)diphthalic anhydride was added to the solution in batches at a uniform interval, and the solution was stirred under gradient vacuum. The gradient vacuum was carried out in six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, and the vacuum rate was 1 ° C / min. Each vacuum process was maintained for 120 min. After stirring for 12 hours, a fluorinated polyamic acid glue solution with a solid content of about 15% was obtained;

[0058] Step 2: Place the fluorinated polyamide acid glue solution in a vacuum oven for degassing treatment, and then coat it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s. Then, it is subjected to microwave-assisted gradient heating thermal imidization treatment with a microwave power of 1000 w. The gradient heating is carried out in seven steps: 60°C → 80°C → 150°C → 200°C → 250°C → 300°C → 350°C. The heating rate is 5°C / min, and the insulation time of each insulation process is 60 min. Finally, a fluorinated polyimide film with a thickness of 10 μm is prepared, which is recorded as F-PI.

[0059] Comparative Example 2

[0060] Step 1: In a 250 ml round-bottom flask, 2.1135 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl was dissolved in 25.0 ml of N,N-dimethylacetamide. Under vacuum, 2.9926 g of 4,4'-(hexafluoroisopropylene)diphthalic anhydride was added to the solution in batches at a uniform interval, and the solution was stirred under gradient vacuum. The gradient vacuum was carried out in six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, and the vacuum rate was 1 ° C / min. Each vacuum process was maintained for 120 min. After stirring for 12 hours, a fluorinated polyamic acid glue solution with a solid content of about 15% was obtained;

[0061] Step 2: Add 0.0085 g of triaminopyrimidine to the fluorinated polyamic acid glue solution, continue to use gradient vacuum stirring, the gradient vacuum is divided into six steps, 25 Pa → 20 Pa → 15 Pa → 10 Pa → 5 Pa → 1 Pa, the vacuum rate is 1 ° C / min, each vacuum process is maintained for 240 min, and after stirring for 24 hours, a slightly cross-linked fluorinated polyamic acid glue solution with a solid content of about 15% is obtained;

[0062] Step three, placing the micro-cross-linked fluorinated polyamide acid glue solution in a vacuum oven for degassing treatment, and then coating it on a glass substrate by a scraping process with a scraping speed of 25 cm / min and a scraping time of 30 s, and then subjected to microwave-assisted gradient heating thermal imidization treatment with a microwave power of 1000 w. The gradient heating is carried out in seven steps, 60°C → 80°C → 150°C → 200°C → 250°C → 300°C → 350°C, with a heating rate of 5°C / min, and the insulation time of each insulation process is 60 min. Finally, a micro-cross-linked fluorinated polyimide film with a thickness of 12 μm is prepared, which is recorded as pyr-0.5 / F-PI.

[0063] Effect example

[0064] The structure and performance of the polyimide-based composite dielectric materials obtained in Examples 1-3 and Comparative Examples 1-2 were characterized, and the results are as follows:

[0065] (1) Figure 3 The XRD patterns of the polyimide-based composite dielectric materials obtained for Examples 1-3 and Comparative Example 1 are as follows: Figure 3 It can be seen that the four fluorinated polyimide composite media show typical "steamed bun-shaped" amorphous diffraction peaks in the diffraction angle range of 10° to 30°, proving that the introduction of the cross-linking agent cage-type octaaminophenylsilsesquioxane has no effect on the crystallinity of the fluorinated polyimide.

[0066] (2) Figure 4 The XRD patterns of the polyimide-based composite dielectric materials obtained for Comparative Example 1 and Comparative Example 2 are as follows: Figure 1It can be seen that the four fluorinated polyimide composite media show typical "steamed bun-shaped" amorphous diffraction peaks in the diffraction angle range of 10° to 30°, proving that the introduction of the cross-linking agent triaminopyrimidine has no effect on the crystallinity of the fluorinated polyimide.

[0067] (3) Figure 5 The infrared spectra comparison diagram of the polyimide-based composite dielectric material obtained by Examples 1-3 and Comparative Example 1; Figure 2 It can be seen that the slightly cross-linked fluorinated polyimide has a peak at 1784 cm -1 The characteristic peak near 1726 cm -1 Symmetrical stretching vibrations of the two carbonyl groups on the imide ring occur at 1377 cm -1 The characteristic peaks at 1784cm-1 in OAPS-0.5 / F-PI correspond to the stretching vibration of CN in the imine ring of fluorinated polyimide. These three characteristic peaks correspond to the characteristic peaks of polyimide, proving that in the process of preparing F-PI, the N atom in the amino group of 2,2'-bis(trifluoromethyl)diaminobenzidine replaced the position of the O atom in -COC- in 4,4'-(hexafluoroisopropylene)diphthalic anhydride, indicating that 4,4'-(hexafluoroisopropylene)diphthalic anhydride and 2,2'-bis(trifluoromethyl)diaminobenzidine successfully reacted. -1 Asymmetric stretching vibration of the carbonyl group of the imide ring nearby at 1726 cm -1 The symmetrical stretching vibration of the two carbonyl groups on the imide ring was significantly weakened, proving that the amino group in the crosslinking agent cage-type octaaminophenylsilsesquioxane reacted with the carboxyl group in the fluorinated polyamic acid to achieve mutual crosslinking.

[0068] (4) Figure 6 The infrared spectrum comparison diagram of the polyimide-based composite dielectric material obtained for Comparative Example 1 and Comparative Example 2; Figure 2 It can be seen that the slightly cross-linked fluorinated polyimide has a peak at 1784 cm -1 The characteristic peak near 1726 cm -1 Symmetrical stretching vibrations of the two carbonyl groups on the imide ring occur at 1377 cm -1 The characteristic peaks at correspond to the stretching vibration of CN of the imine ring of fluorinated polyimide. These three characteristic peaks correspond to the characteristic peaks of polyimide, proving that in the process of preparing F-PI, the N atom in the amino group of 2,2'-bis(trifluoromethyl)diaminobenzidine replaced the position of the O atom in -COC- in 4,4'-(hexafluoroisopropylene)diphthalic anhydride, indicating that 4,4'-(hexafluoroisopropylene)diphthalic anhydride successfully reacted with 2,2'-bis(trifluoromethyl)diaminobenzidine, and the introduction of the crosslinker did not affect the imidization process of polyimide. At the same time, it can be seen that at pyr-0.5 / F-PI 1377cm-1 The stretching vibration peak of CN of the nearby imide imide ring is enhanced, proving that triaminopyrimidine reacts with fluorinated polyamic acid, an amide bond is formed between the amino group and the carboxyl group, and a cross-linking reaction occurs, thereby forming a cross-linked structure.

[0069] (5) Figure 7 and Figure 8 The discharge energy density and charge-discharge efficiency of the polyimide-based insulating medium prepared in Example 2, Comparative Example 1 and Comparative Example 2 at 150°C are shown as a function of the field strength. Figure 7 It can be seen that the cross-linked structure can significantly improve the energy storage density of the fluorinated polyimide composite dielectric. The energy storage density of the OAPS-0.5 / F-PI composite dielectric prepared in Example 2 is 4.18 J / cm at 150 °C and 580 MV / m. 3 , which is 40% higher than that of F-PI dielectric material and 18% higher than that of pyr-0.5 / F-PI composite dielectric. Figure 6 It can be seen that at 150°C, the energy storage efficiency of the OAPS-0.5 / F-PI composite medium prepared in Example 2 is still maintained at more than 90% at 580MV / m. This is because the cage-type octaaminophenylsilsesquioxane itself is a three-dimensional structure, which contains multiple cross-linking points, thereby forming a stable three-dimensional network structure. The segment structure is not easy to break under strong impact, which enhances the intermolecular force between the chains. At the same time, the introduction of silicon elements can also increase the flexibility and heat resistance of the material.

[0070] Although the present invention has been disclosed as above in the preferred embodiments, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing a cross-linked polyimide insulating medium, characterized in that: Prepared by the following steps: (1) Under vacuum conditions, fluorinated polyamic acid adhesive is prepared by polycondensation of fluorinated diamine and fluorinated dianhydride; The molar ratio of the fluorinated diamine to the fluorinated dianhydride in (1) is (1-1.08): (1.02-1.2); the mass fractions of the fluorinated diamine and the fluorinated dianhydride in the polycondensation system are both 12%-35%; the fluorinated diamine is 2,2'-bis(trifluoromethyl)diaminobiphenyl, and the fluorinated dianhydride is 4,4'-(hexafluoroisopropylene) diphthalic anhydride; (2) under vacuum conditions, adding a crosslinking agent to the fluorinated polyamic acid glue solution and stirring to obtain a slightly crosslinked fluorinated polyamic acid glue solution; The crosslinking agent in (2) is 2,4,6-triaminopyrimidine, and the content of amino groups added to the crosslinking agent is 0.1% to 10% of the total molar amount of amino groups in the fluorinated diamine; (3) A coating method is adopted to prepare a wet film using a slightly cross-linked fluorinated polyamide acid adhesive solution, and the wet film is subjected to microwave-assisted thermal imidization treatment to obtain a cross-linked polyimide insulating dielectric film.

2. The preparation method according to claim 1, characterized in that: (1) The polycondensation reaction temperature is -10 to 40°C and the reaction time is 2 to 24 hours.

3. The preparation method according to claim 1, characterized in that: The vacuum conditions in (1) and (2) are achieved by a step vacuum method, wherein the vacuum gradient interval of each step vacuum is 1-5 Pa, the vacuum rate is 1-2 Pa / min, and the constant vacuum time of each step is 30-180 min.

4. The preparation method according to claim 1, characterized in that: (3) The microwave-assisted thermal imidization treatment conditions are as follows: microwave power is 1000W~5000W, thermal imidization is gradient heating, each temperature gradient interval of the gradient heating is 20~100℃, the heating rate is 3~15℃ / min, and the constant temperature time of each section is 30~720min.

5. A cross-linked polyimide insulating dielectric film obtained by the preparation method according to any one of claims 1 to 4, characterized in that: The film thickness is 3~20μm.

6. An application of the cross-linked polyimide insulating dielectric film according to claim 5, characterized in that: Used in the preparation of electrical insulation devices.