A silane cross-linked polyethylene cable insulation material and preparation method thereof

By using epoxy castor oil and organically modified silica in silane cross-linked polyethylene cable insulation material to form a bridge chain structure, combined with the rigidity and toughening of nano-silica, the brittleness of cross-linked polyethylene materials at low temperatures is solved. problem, significantly improving cold resistance performance.

CN117801406BActive Publication Date: 2024-10-22SUZHOU HENGLI COMM MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311829628.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-10-22
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

Cross-linked polyethylene materials are prone to low-temperature brittleness at low temperatures and lack cold resistance.

Method used

A toughening agent is introduced into the silane cross-linked polyethylene cable insulation material, and a bridge chain structure is formed through the ring-opening grafting reaction of epoxy castor oil and organically modified silica. Combined with the rigidity and toughening effect of nano-silica, it improves the The cold resistance of the material.

Benefits of technology

The cold-resistant performance of silane cross-linked polyethylene cable insulation material is significantly improved, the problem of low-temperature brittleness is solved, and a dual toughening effect is achieved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a silane cross-linked polyethylene cable insulation material and a preparation method, and belongs to the technical field of insulating material preparation. The silane cross-linked polyethylene cable insulation material comprises the following raw materials in parts by weight: 70-95 parts of polyethylene, 2-4 parts of vinyl silane, 0.05-0.4 parts of water-generating agent, 0.1-1 parts of antioxidant and 0.1-1 parts of catalyst, and is characterized in that it also comprises 15-25 parts by weight of toughening agent; the toughening agent is formed by ring-opening grafting reaction of epoxy castor oil and organic modified silica in a mixed solvent; wherein the mixed solvent is a mixture of water and ethanol; the organic modified silica is prepared by surface modification reaction of aminosilane coupling agent and silica. The present invention introduces a toughening agent into the silane cross-linked polyethylene cable insulation material to improve the cold resistance of the obtained silane cross-linked polyethylene cable insulation material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of insulating material preparation, and particularly relates to a silane cross-linked polyethylene cable insulating material and a preparation method thereof. Background Art

[0002] Cross-linked polyethylene materials have excellent electrical and mechanical properties due to their unique three-dimensional network structure consisting of polyethylene polymer chains grafted with vinyl silane branches, making them gradually widely used in cable insulation materials. However, since the main molecular chains of the three-dimensional network structure of cross-linked polyethylene materials are polyethylene polymer chains, they inevitably lack low temperature resistance and are prone to low-temperature brittleness at low temperatures. Summary of the invention

[0003] In view of the above problems, the present invention provides a silane cross-linked polyethylene cable insulation material and a preparation method thereof.

[0004] The first object of the present invention is to provide a silane cross-linked polyethylene cable insulation material, comprising the following raw materials in parts by weight: 70-95 parts of polyethylene, 2-4 parts of vinyl silane, 0.05-0.4 parts of water generating agent, 0.1-1 parts of antioxidant, 0.1-1 parts of catalyst and 15-25 parts of toughening agent;

[0005] In an embodiment of the present invention, the toughening agent is formed by ring-opening grafting reaction of epoxy castor oil and organic modified silica in a mixed solvent;

[0006] Wherein, the mixed solvent is a mixture of water and ethanol;

[0007] The organic modified silicon dioxide is prepared by surface modification reaction of an aminosilane coupling agent and silicon dioxide, and the particle size of the silicon dioxide is 200-600nm.

[0008] In an embodiment of the present invention, the polyethylene is composed of a mixture of low-density polyethylene and high-density polyethylene in a mass ratio of 10:0.5-3.

[0009] In an embodiment of the present invention, in the ring-opening grafting reaction, the mass ratio of the epoxy castor oil to the organic modified silica is 10:1.2-3.1.

[0010] In the embodiment of the present invention, the reaction temperature of the ring-opening grafting reaction is 60-75° C., and the reaction time is 1-24 h.

[0011] In an embodiment of the present invention, the volume ratio of water to ethanol in the mixed solvent is 10:1-3.

[0012] In an embodiment of the present invention, the reaction solvent of the surface modification reaction is a mixture of water and ethanol in a volume ratio of 0.1-2:10.

[0013] In the embodiment of the present invention, the mass ratio of aminosilane coupling agent to silicon dioxide in the surface modification reaction is 4-6:10, the reaction temperature is 50-70° C., and the reaction time is 3-10 h.

[0014] In an embodiment of the present invention, the epoxy castor oil is prepared by catalytic oxidation of castor oil and urea in glacial acetic acid with acidic aluminum oxide and hydrogen peroxide.

[0015] In an embodiment of the present invention, the reaction temperature of the catalytic oxidation is 60-65° C., the reaction time is 12-24 hours, and the mass ratio of the castor oil to the urea is 10:0.3-1.

[0016] In the embodiment of the present invention, the vinyl silane is a mixture of vinyl trimethoxyethoxy silane and vinyl trimethoxy silane in any ratio.

[0017] In an embodiment of the present invention, the water producing agent is zinc acetate.

[0018] In the embodiment of the present invention, the antioxidant is one or a mixture of several of the antioxidant HP-136, antioxidant 1024, antioxidant 925, antioxidant 1010, antioxidant DSTP, antioxidant 168 and antioxidant DLTP.

[0019] In an embodiment of the present invention, the catalyst is an organic tin, such as dibutyltin dilaurate.

[0020] The second object of the present invention is to provide a method for preparing a silane cross-linked polyethylene cable insulation material, comprising:

[0021] After the vinyl silane and the first part of polyethylene are uniformly mixed, they are added into an extruder and extruded into pellets to obtain first pellets;

[0022] The first pellet, the second part of polyethylene, the water generating agent, the antioxidant, the catalyst and the toughening agent are mixed evenly, added into the extruder, and extruded and granulated to obtain the cable insulation material.

[0023] The first part of polyethylene and the second part of polyethylene constitute the raw material of polyethylene, and the mass ratio of the first part of polyethylene to the second part of polyethylene is 0.1-0.3:10.

[0024] Beneficial effects of the present invention:

[0025] In order to solve the problems in the background technology, the present invention introduces a toughening agent into a silane cross-linked polyethylene cable insulation material, and the toughening agent is a core-shell composite composed of organic and inorganic substances, wherein the core is nano-silicon dioxide, which is a common rigid toughening particle, and the shell is a castor oil molecular chain, which is a commonly used environmentally friendly toughening agent. The two are chemically reacted to form a bridge chain between the two, which can solve the agglomeration problem of nano-particles and the migration problem of castor oil, and can achieve the dual toughening effect of toughening rigid particles and toughening castor oil, thereby improving the cold resistance of the obtained silane cross-linked polyethylene cable insulation material;

[0026] In the present invention, the molecular chain of the bridge chain is formed by the reaction of aminosiloxane core epoxy groups, wherein the siloxane chain has good flexibility and can form good interaction with the three branches of epoxy castor oil, thereby improving the grafting rate of castor oil and nano-silicon dioxide;

[0027] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and claims. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] A silane cross-linked polyethylene cable insulation material according to an embodiment of the present invention comprises the following raw materials in parts by weight: 70-95 parts of polyethylene, 2-4 parts of vinyl silane, 0.05-0.4 parts of a water generating agent, 0.1-1 parts of an antioxidant, 0.1-1 parts of a catalyst and 15-25 parts of a toughening agent;

[0030] The toughening agent is formed by ring-opening grafting reaction of epoxy castor oil and organic modified silica in a mixed solvent, wherein the mixed solvent is a mixture of water and ethanol, and the organic modified silica is prepared by surface modification reaction of an aminosilane coupling agent and silica, and the aminosilane coupling agent is an aminosilane coupling agent well known in the technical field, such as KH-570, KH-792, KH-602, etc., and the particle size of silica is 200-600nm.

[0031] In the embodiment of the present invention, the raw material ratio of the silane cross-linked polyethylene cable insulation material is any one of the formulas in Table 1:

[0032] Table 1 (parts by weight)

[0033] Recipe No. Polyethylene Vinyl Silicone Water producing agent Antioxidants catalyst Toughening agent 1 95 2 0.05 0.1 0.1 15 2 90 3 0.1 0.5 0.5 16 3 90 4 0.4 1 1 18 4 80 2 0.08 0.2 0.4 18 5 80 3 0.2 0.5 0.5 20 6 85 4 0.4 1 1 20 7 75 2 0.07 0.2 0.4 20 8 75 3 0.2 0.5 0.5 25 9 70 4 0.4 1 1 25

[0034] In the embodiment of the present invention, the polyethylene is composed of low-density polyethylene and high-density polyethylene mixed in a mass ratio of 10:0.5-3, utilizing the good grafting and mixed modification characteristics of low-density polyethylene, introducing high-density polyethylene, and utilizing the excellent cold resistance of high-density polyethylene to improve the cold resistance of the overall polyethylene system;

[0035] The specific values ​​of the mass ratio of the low-density polyethylene to the high-density polyethylene are 10:0.5, 10:1, 10:1.5, 10:2, 10:2.5 or 10:3.

[0036] In the embodiment of the present invention, in the ring-opening grafting reaction, the mass ratio of the epoxy castor oil to the organic modified silica is 10:1.2-3.1;

[0037] The specific value of the mass ratio of the oxygen castor oil and the organic modified silica is 10:1.2, 10:1.3, 10:1.4, 10:1.5, 10:1.6, 10:1.7, 10:1.8, 10:1.9, 10:2.0, 10:2.1, 10:2.2, 10:2.3, 10:2.4, 10:2.5, 10:2.6, 10:2.7, 10:2.8, 10:2.9 or 10:3;

[0038] The reaction temperature of the ring-opening grafting reaction is 60-75°C, and the reaction time is 1-24h;

[0039] The reaction temperature of the ring-opening grafting reaction is 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 67°C, 70°C, 71°C, 72°C, 73°C, 74°C or 75°C;

[0040] The reaction time of the ring-opening grafting reaction is 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, 21 h, 22 h, 23 h or 24 h.

[0041] The volume ratio of water to ethanol in the mixed solvent is 10:1-3, and the specific volume ratio is 10:1, 10:1.1, 10:1.2, 10:1.3, 10:1.4, 10:1.5, 10:1.6, 10:1.7, 10:1.8, 10:1.9, 10:2, 10:2.1, 10:2.2, 10:2.3, 10:2.4, 10:2.5, 10:2.6, 10:2.7, 10:2.8, 10:2.9 or 10:3.

[0042] In an embodiment of the present invention, the reaction solvent of the surface modification reaction is a mixture of water and ethanol in a volume ratio of 0.1-2:10, and the specific volume ratio is 0.1:10, 0.2:10, 0.3:10, 0.4:10, 0.5:10, 0.6:10, 0.7:10, 0.8:10, 0.9:10, 1.0:10, 1.1:10, 1.2:10, 1.3:10, 1.4:10, 1.5:10, 1.6:10, 1.7:10, 1.8:10, 1.9:10 or 2.0:10.

[0043] In the embodiment of the present invention, the mass ratio of aminosilane coupling agent to silicon dioxide in the surface modification reaction is 4-6:10, the reaction temperature is 50-70° C., and the reaction time is 3-10 h;

[0044] The specific value of the mass ratio of the aminosilane coupling agent to silicon dioxide is 4:10, 4.1:10, 4.2:10, 4.3:10, 4.4:10, 4.5:10, 4.6:10, 4.7:10, 4.8:10, 4.9:10, 5.0:10, 5.1:10, 5.2:10, 5.3:10, 5.4:10, 5.5:10, 5.6:10, 5.7:10, 5.8:10, 5.9:10 or 6:10;

[0045] The reaction temperature of the surface modification reaction is 50°C, 55°C, 60°C, 65°C or 70°C;

[0046] The reaction time of the surface modification reaction is 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h.

[0047] In an embodiment of the present invention, the epoxy castor oil is prepared by catalytic oxidation of castor oil and urea in glacial acetic acid with acidic aluminum oxide and hydrogen peroxide;

[0048] Specifically, the reaction temperature of the catalytic oxidation is 60-65°C, the reaction time is 12-24h, the mass ratio of the castor oil to the urea is 10:0.3-1, the amount of the acidic alumina is 2-6% of the total mass of the castor oil and urea, and the amount of the hydrogen peroxide is 1-3% of the total mass of the castor oil and urea;

[0049] The mass ratio of castor oil to urea is 10:0.3, 10:0.4, 10:0.5, 10:0.6, 10:0.7, 10:0.8, 10:0.9 or 10:1;

[0050] The reaction temperature and reaction time of the catalytic oxidation are 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h or 24h.

[0051] The preparation of the silane cross-linked polyethylene cable insulation material and its physical property test are given as an example below:

[0052] 1. Preparation of reaction raw materials: Example 1

[0053] Preparation of Epoxidized Castor Oil:

[0054] Add 100g castor oil and 6g urea to 150mL glacial acetic acid, stir for 10-20min, then add 7g acidic alumina, continue stirring for 10-20min, heat to the reaction system temperature of 55°C, then slowly add 30wt% 50g hydrogen peroxide solution under stirring, after complete addition, heat to 60°C, stir and react for 12h, stop the reaction, separate the liquids, wash the oil layer, and then evaporate under reduced pressure to obtain epoxy castor oil. Example 2

[0055] Preparation of organic modified silica:

[0056] 10 g of silica was added to 60 mL of a solvent formed by mixing water and ethanol (water and ethanol in a volume ratio of 0.1:10), and after stirring and mixing evenly, the reaction system temperature was heated to 70°C, and 5 g of an aminosilane coupling agent was slowly added dropwise under stirring. After the addition was complete, the reaction was continued to be kept warm for 8 hours, filtered, and washed to obtain modified silica, wherein the aminosilane coupling agent was KH570. Example 3

[0057] Preparation of toughening agent:

[0058] 100 g of the epoxy castor oil prepared in Example 1 and 25 g of the organic modified silica prepared in Example 2 were added to 150 mL of a mixed solvent formed by mixing water and ethanol in a volume ratio of 10:1, stirred evenly, heated to 65° C., stirred and reacted for 16 hours, stopped the reaction, filtered, washed with water and ethanol, and obtained a toughening agent.

[0059] Comparative Example 1

[0060] Preparation of toughening agent:

[0061] 100 g of the epoxy castor oil prepared in Example 1 and 25 g of silicon dioxide were added to 150 mL of a mixed solvent formed by mixing water and ethanol in a volume ratio of 10:1, stirred evenly, heated to 65° C., stirred and reacted for 16 hours, stopped the reaction, filtered, washed with water and ethanol, and obtained a toughening agent.

[0062] 2. Finished product preparation:

[0063] Example 4

[0064] Step 1: Prepare the raw materials according to Table 1;

[0065] Wherein, the polyethylene is composed of a mixture of low-density polyethylene and high-density polyethylene in a mass ratio of 10:2;

[0066] The water producing agent is zinc acetate;

[0067] The antioxidant is antioxidant 1024;

[0068] The catalyst is dibutyltin dilaurate;

[0069] The toughening agent is prepared according to Example 3;

[0070] Step 2: After the vinyl silane and the first part of polyethylene are uniformly mixed, they are added into an extruder and extruded into granules to obtain first granules;

[0071] The third step is to mix the first pellet, the second part of polyethylene, the water producing agent, the antioxidant, the catalyst and the toughening agent evenly, add them into the extruder, and granulate them by extrusion to obtain the cable insulation materials labeled as Example 4-1, Example 4-2, Example 4-3, Example 4-4, Example 4-5, Example 4-6, Example 4-7, Example 4-8 and Example 4-9. The raw material ratios of the cable insulation materials of Example 4-1, Example 4-2, Example 4-3, Example 4-4, Example 4-5, Example 4-6, Example 4-7, Example 4-8 and Example 4-9 correspond to the serial numbers in Table 1;

[0072] The first part of polyethylene and the second part of polyethylene constitute the raw material of polyethylene, and the mass ratio of the first part of polyethylene to the second part of polyethylene is 0.1:10.

[0073] Comparative Example 2

[0074] Step 1: Prepare the raw materials according to the ingredients numbered 2, 5, and 8 in Table 1;

[0075] Wherein, the polyethylene is composed of a mixture of low-density polyethylene and high-density polyethylene in a mass ratio of 10:2;

[0076] The water producing agent is zinc acetate;

[0077] The antioxidant is antioxidant 1024;

[0078] The catalyst is dibutyltin dilaurate;

[0079] The toughening agent is prepared according to Comparative Example 1;

[0080] The second and third steps are the same as those in Example 4;

[0081] The obtained cable insulation materials are Comparative Example 2-2, Comparative Example 2-5, and Comparative Example 2-8.

[0082] Comparative Example 3

[0083] The first step is to delete the toughening agent in the ingredients numbered 2, 5, and 8 in Table 1, and then prepare the raw materials;

[0084] Wherein, the polyethylene is composed of a mixture of low-density polyethylene and high-density polyethylene in a mass ratio of 10:2;

[0085] The water producing agent is zinc acetate;

[0086] The antioxidant is antioxidant 1024;

[0087] The catalyst is dibutyltin dilaurate;

[0088] The second and third steps are the same as those in Example 4;

[0089] The obtained cable insulation materials are Comparative Example 3-2, Comparative Example 3-5, Comparative Example 3-8

[0090] The cable insulation materials obtained in Example 4, Comparative Example 2 and Comparative Example 3 were made into test samples, and the tensile properties and gel content (content after being placed at 25°C for two days) were tested according to the test method in JB / T 10437, and the low-temperature brittle temperature was tested according to GB / T 5470, and the test conditions were -40°C, 3min. The above test results are shown in Table 2;

[0091] Table 2

[0092] Tensile Strength Elongation at break Gel content Low temperature embrittlement temperature unit Mpa % wt% ℃ Example 4-1 17.2 411 64.1 -40 Example 4-2 17.4 416 66.2 -42 Example 4-3 17.7 420 69.4 -44 Example 4-4 18.1 423 69.5 -45 Embodiment 4-5 19.2 431 70.1 -48 Embodiment 4-6 20.1 443 72.5 -45 Embodiment 4-7 20.4 452 74.8 -53 Embodiment 4-8 21.3 459 76.2 -56 Embodiment 4-9 21.1 476 77.6 -60 Comparative Example 2-2 16.1 347 66.1 -25 Comparative Examples 2-5 17.9 351 69.5 -27 Comparative Examples 2-8 18.8 310 75.4 -28 Comparative Example 3-2 13.1 323 65.5 -20 Comparative Examples 3-5 12.7 324 65.7 -20 Comparative Examples 3-8 13.3 323 65.8 -20

[0093] It can be seen from the data in Table 2 that the cable insulation material obtained in Example 4 has good cold resistance.

[0094] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A silane cross-linked polyethylene cable insulation material, comprising the following raw materials in parts by weight: 70-95 parts of polyethylene, 2-4 parts of vinyl silane, 0.05-0.4 parts of water generating agent, 0.1-1 parts of antioxidant and 0.1-1 parts of catalyst, characterized in that: Also includes 15-25 parts by weight of toughening agent; The toughening agent is formed by ring-opening grafting reaction of epoxy castor oil and organic modified silica in a mixed solvent; Wherein, the mixed solvent is a mixture of water and ethanol; The organic modified silica is prepared by surface modification reaction of an aminosilane coupling agent and silica; The mass ratio of the epoxy castor oil to the organic modified silica in the ring-opening grafting reaction is 10:1.2-3.1; The reaction temperature in the ring-opening grafting reaction is 60-75°C and the reaction time is 1-24h; The volume ratio of water to ethanol in the mixed solvent is 10:1-3; The reaction solvent in the surface modification reaction is a mixture of water and ethanol in a volume ratio of 0.1-2:10; In the surface modification reaction, the mass ratio of the aminosilane coupling agent to silicon dioxide is 4-6:10, the reaction temperature is 50-70° C., and the reaction time is 3-10 hours.

2. The silane cross-linked polyethylene cable insulation material according to claim 1, characterized in that: The polyethylene is composed of a mixture of low-density polyethylene and high-density polyethylene in a mass ratio of 10:0.5-3.

3. The silane cross-linked polyethylene cable insulation material according to claim 1, characterized in that: The epoxy castor oil is prepared by catalytic oxidation of castor oil and urea in glacial acetic acid with acidic aluminum oxide and hydrogen peroxide.

4. The silane cross-linked polyethylene cable insulation material according to claim 3, characterized in that: The reaction temperature of the catalytic oxidation is 60-65° C., the reaction time is 12-24 hours, and the mass ratio of castor oil to urea is 10:0.3-1.

5. The method for preparing the silane cross-linked polyethylene cable insulation material according to any one of claims 1 to 4, characterized in that: include: After the vinyl silane and the first part of polyethylene are uniformly mixed, they are added into an extruder and extruded into pellets to obtain first pellets; The first pellet, the second part of polyethylene, the water generating agent, the antioxidant, the catalyst and the toughening agent are mixed evenly, added into the extruder, and extruded and granulated to obtain the cable insulation material. The first part of polyethylene and the second part of polyethylene constitute the raw material of polyethylene, and the mass ratio of the first part of polyethylene to the second part of polyethylene is 0.1-0.3:10.