A wear-resistant and tear-resistant optical cable material and preparation method thereof
By combining the modified boron nitride compound with the base material in the optical cable material, the wear resistance and mechanical properties of the optical cable material are improved, the problem of insufficient wear resistance of the existing optical cable material is solved, and higher resistance is achieved. Wear and tear resistance.
Patent Information
- Application Number
- CN202311843537.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-29
AI Technical Summary
The wear resistance of existing optical cable materials is insufficient, especially the mechanical properties and aging resistance of sheath materials need to be further improved.
It uses components such as low-density polyethylene, ethylene-vinyl acetate copolymer, modified boron nitride compound, calcium stearate, expandable graphite powder, zinc stannate and polyethylene wax, and is processed through ultrasonic dispersion and ball milling. Nano-silica doped hexagonal boron nitride powder is prepared through freeze-drying, grinding and high-temperature sintering steps, and is combined with the base material to improve the mechanical properties of the optical cable material.
It significantly improves the wear resistance and mechanical properties of the optical cable material, enhances its wear resistance and tear resistance, and shows better density and porosity than materials directly added with hexagonal boron nitride.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical cable material preparation, and in particular to a wear-resistant and tear-resistant optical cable material and a preparation method thereof. Background Art
[0002] Optical cable materials refer to materials that can transmit optical signals, mainly composed of glass fiber and plastic. Glass fiber is the main material of optical cable, which has the characteristics of anti-interference, fast transmission speed, high bandwidth, low optical loss, high signal fidelity, and excellent corrosion resistance, heat resistance and radiation resistance. In addition to optical fiber, optical cable also includes other materials, such as plastic protective layer, metal sheath, insulating material, etc. The function of these materials is to protect the optical fiber and improve the durability and performance of the optical cable.
[0003] As the protective layer of the optical cable material, the plastic protective layer has a great influence on the comprehensive performance of the optical cable. It is not only required to have excellent physical properties, such as tensile strength, elongation at break, etc., but also needs to have good wear resistance and aging resistance. Although there are many kinds of optical cables on the market, the performance of most sheath materials is still not very ideal. For example, Chinese patent document CN202011348470.9 discloses a low-smoke halogen-free cable material and its preparation method and application. The low-smoke halogen-free cable comprises the following components in parts by weight: 10 to 30 parts by weight of high-density polyethylene, 5 to 20 parts by weight of thermoplastic elastomer, 0.5 to 10 parts by weight of ethylene propylene rubber, 30 to 40 parts by weight of aluminum hydroxide, and 2 to 10 parts by weight of magnesium aluminum hydrotalcite. Although the prepared low-smoke halogen-free cable material has good flame retardant and mechanical properties, its wear resistance still needs to be further improved. Summary of the invention
[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide a wear-resistant and tear-resistant optical cable material and a preparation method thereof, wherein the prepared material has good mechanical properties and wear resistance.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme:
[0006] A wear-resistant and tear-resistant optical cable material comprises the following raw materials, measured by weight: 40-60 parts of low-density polyethylene, 5-10 parts of ethylene-vinyl acetate copolymer, 10-15 parts of modified boron nitride compound, 1-2 parts of calcium stearate, 3-5 parts of expandable graphite powder, 0.5-1 parts of zinc stannate, 0.4-0.8 parts of polyethylene wax and 5-8 parts of compatibilizer.
[0007] Preferably, the preparation method of the modified boron nitride composite is as follows:
[0008] S1, immersing hexagonal boron nitride and nano-silicon dioxide in anhydrous ethanol, uniformly dispersing by ultrasonication, and then ball-milling, freeze-drying, grinding, sieving, high-temperature sintering, crushing and grading the ball-milled slurry, and then passing through a 400-mesh sieve to obtain a mixed powder;
[0009] S2. Add stearic acid to anhydrous methanol solvent, heat and stir to dissolve, then add the mixed powder, continue stirring for 4-8 hours, filter the resulting suspension, wash and dry to obtain a modified boron nitride composite.
[0010] Preferably, in step S1, the mass ratio of hexagonal boron nitride to nano-silicon dioxide is 10-15:2-3.
[0011] Preferably, in step S1, the ball milling treatment time is 3-6 hours.
[0012] Preferably, in step S1, the high temperature sintering temperature is 1400-1600° C., and the high temperature sintering time is 2-3 hours.
[0013] Preferably, in step S2, the mass ratio of stearic acid, anhydrous methanol and mixed powder is 1-2:100:10-20.
[0014] Preferably, in step S2, the temperature of heating and stirring is 55-65°C.
[0015] Preferably, the compatibilizer is selected from POE-g-MAH or EVA-g-MAH.
[0016] The present invention also provides a method for preparing the above-mentioned wear-resistant and tear-resistant optical cable material, comprising the following steps: weighing low-density polyethylene, ethylene-vinyl acetate copolymer, modified boron nitride composite, calcium stearate, expandable graphite powder, zinc stannate, polyethylene wax and compatibilizer by weight, mixing all the raw materials evenly and kneading for 2-3 minutes, and then transferring them to a twin-screw extruder for extrusion granulation to obtain the wear-resistant and tear-resistant optical cable material.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present invention compounds hexagonal boron nitride and nano-silicon dioxide for the first time to prepare nano-silicon dioxide-doped hexagonal boron nitride mixed powder, which has the characteristics of good density and small porosity. Compared with directly adding hexagonal boron nitride to a substrate, the optical cable material prepared by the present invention has more excellent wear resistance.
[0019] The present invention utilizes stearic acid to perform surface modification on nano silicon dioxide doped hexagonal boron nitride powder, and adds the surface modified powder into a substrate, thereby improving the compatibility between the nano silicon dioxide doped hexagonal boron nitride powder and the substrate, and further improving the mechanical properties of the optical cable material. DETAILED DESCRIPTION
[0020] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.
[0021] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.
[0022] The low-density polyethylene used in the present invention was purchased from Suzhou Longou Plastic Chemical Co., Ltd., item number: DJ210;
[0023] Ethylene-vinyl acetate copolymer was purchased from Ningbo Baofuyi New Materials Co., Ltd., item number: 28-150;
[0024] Hexagonal boron nitride was purchased from Beasley New Materials (Suzhou) Co., Ltd., CAS: 10043-11-5;
[0025] The particle size of nano-silicon dioxide is 20-40nm;
[0026] Expandable graphite powder was purchased from Shandong Xiangzhao New Materials Co., Ltd., item number: KPZSM1104.
[0027] Example 1
[0028] A method for preparing a wear-resistant and tear-resistant optical cable material comprises the following steps:
[0029] 60 parts of low-density polyethylene, 5 parts of ethylene-vinyl acetate copolymer, 10 parts of modified boron nitride composite, 1 part of calcium stearate, 3 parts of expandable graphite powder, 0.5 parts of zinc stannate, 0.6 parts of polyethylene wax and 5 parts of compatibilizer POE-g-MAH were mixed uniformly, first kneaded at 160°C for 3 minutes, and then transferred to a twin-screw extruder for extrusion granulation to obtain a wear-resistant and tear-resistant optical cable material;
[0030] Wherein, the preparation method of the modified boron nitride composite is as follows:
[0031] S1. Immerse 10g of hexagonal boron nitride and 2g of nano-silicon dioxide in 150mL of anhydrous ethanol, disperse them uniformly by ultrasonication, and then perform ball milling for 3h. The ball milled slurry is freeze-dried, ground, and sieved. The sintered body is sintered at 1550°C for 2h. The sintered body is placed in a diamond crushing and grading equipment for crushing and grading, and passed through a 400-mesh sieve to obtain a mixed powder.
[0032] S2. Add 1 g of stearic acid to 100 g of anhydrous methanol solvent, heat and stir at 55°C to dissolve, then add 10 g of the mixed powder, continue stirring for 4 hours, filter the resulting suspension, wash and dry to obtain a modified boron nitride composite.
[0033] Example 2
[0034] A method for preparing a wear-resistant and tear-resistant optical cable material comprises the following steps:
[0035] 40 parts of low-density polyethylene, 10 parts of ethylene-vinyl acetate copolymer, 15 parts of modified boron nitride composite, 2 parts of calcium stearate, 4 parts of expandable graphite powder, 0.8 parts of zinc stannate, 0.4 parts of polyethylene wax and 6 parts of compatibilizer POE-g-MAH were mixed uniformly, first kneaded at 160° C. for 2 minutes, and then transferred to a twin-screw extruder for extrusion granulation to obtain a wear-resistant and tear-resistant optical cable material;
[0036] Wherein, the preparation method of the modified boron nitride composite is as follows:
[0037] S1. Immerse 15g of hexagonal boron nitride and 3g of nano-silicon dioxide in 150mL of anhydrous ethanol, disperse them uniformly by ultrasonication, and then perform ball milling for 6h. The ball milled slurry is freeze-dried, ground, and sieved. The sintered body is sintered at 1600°C for 3h. The sintered body is placed in a diamond crushing and grading equipment for crushing and grading, and passed through a 400-mesh sieve to obtain a mixed powder.
[0038] S2. Add 2 g of stearic acid to 100 g of anhydrous methanol solvent, heat and stir at 60°C to dissolve, then add 10 g of the mixed powder, continue stirring for 6 hours, filter the resulting suspension, wash and dry to obtain a modified boron nitride composite.
[0039] Example 3
[0040] A method for preparing a wear-resistant and tear-resistant optical cable material comprises the following steps:
[0041] 50 parts of low-density polyethylene, 6 parts of ethylene-vinyl acetate copolymer, 12 parts of modified boron nitride composite, 1.5 parts of calcium stearate, 5 parts of expandable graphite powder, 1 part of zinc stannate, 0.8 parts of polyethylene wax and 8 parts of compatibilizer EVA-g-MAH were mixed uniformly, first kneaded at 160° C. for 2 minutes, and then transferred to a twin-screw extruder for extrusion granulation to obtain a wear-resistant and tear-resistant optical cable material;
[0042] Wherein, the preparation method of the modified boron nitride composite is as follows:
[0043] S1. Immerse 12g of hexagonal boron nitride and 3g of nano-silicon dioxide in 150mL of anhydrous ethanol, disperse them uniformly by ultrasonication, and then perform ball milling for 5h. The ball milled slurry is freeze-dried, ground, and sieved. The sintered body is sintered at 1400°C for 3h. The sintered body is placed in a diamond crushing and grading equipment for crushing and grading, and passed through a 400-mesh sieve to obtain a mixed powder.
[0044] S2. Add 2 g of stearic acid to 100 g of anhydrous methanol solvent, heat and stir at 60°C to dissolve, then add 20 g of the mixed powder, continue stirring for 8 hours, filter the resulting suspension, wash and dry to obtain a modified boron nitride composite.
[0045] Example 4
[0046] A method for preparing a wear-resistant and tear-resistant optical cable material comprises the following steps:
[0047] 45 parts of low-density polyethylene, 10 parts of ethylene-vinyl acetate copolymer, 10 parts of modified boron nitride composite, 1 part of calcium stearate, 3 parts of expandable graphite powder, 0.8 parts of zinc stannate, 0.5 parts of polyethylene wax and 6 parts of compatibilizer EVA-g-MAH were mixed uniformly, first kneaded at 160° C. for 2 minutes, and then transferred to a twin-screw extruder for extrusion granulation to obtain a wear-resistant and tear-resistant optical cable material;
[0048] Wherein, the preparation method of the modified boron nitride composite is as follows:
[0049] S1. Immerse 15g of hexagonal boron nitride and 3g of nano-silicon dioxide in 150mL of anhydrous ethanol, disperse them uniformly by ultrasonication, and then perform ball milling for 5h. The ball milled slurry is freeze-dried, ground, and sieved. The sintered body is sintered at 1400°C for 3h. The sintered body is placed in a diamond crushing and grading equipment for crushing and grading, and passed through a 400-mesh sieve to obtain a mixed powder.
[0050] S2. Add 2 g of stearic acid to 100 g of anhydrous methanol solvent, heat and stir at 60°C to dissolve, then add 16 g of the mixed powder, continue stirring for 8 hours, filter the resulting suspension, wash and dry to obtain a modified boron nitride composite.
[0051] Comparative Example 1
[0052] A method for preparing a wear-resistant and tear-resistant optical cable material comprises the following steps:
[0053] 40 parts of low-density polyethylene, 10 parts of ethylene-vinyl acetate copolymer, 15 parts of modified boron nitride composite, 2 parts of calcium stearate, 4 parts of expandable graphite powder, 0.8 parts of zinc stannate, 0.4 parts of polyethylene wax and 6 parts of compatibilizer POE-g-MAH were mixed uniformly, first kneaded at 160° C. for 2 minutes, and then transferred to a twin-screw extruder for extrusion granulation to obtain a wear-resistant and tear-resistant optical cable material;
[0054] Wherein, the preparation method of the modified boron nitride composite is as follows:
[0055] 2 g of stearic acid was added to 100 g of anhydrous methanol solvent, heated and stirred at 60°C to dissolve, and then 10 g of hexagonal boron nitride was added thereto, and stirring was continued for 6 hours. The obtained suspension was filtered, washed, and dried to obtain a modified boron nitride composite.
[0056] Comparative Example 2
[0057] A method for preparing a wear-resistant and tear-resistant optical cable material comprises the following steps:
[0058] 40 parts of low-density polyethylene, 10 parts of ethylene-vinyl acetate copolymer, 15 parts of modified boron nitride composite, 2 parts of calcium stearate, 4 parts of expandable graphite powder, 0.8 parts of zinc stannate, 0.4 parts of polyethylene wax and 6 parts of compatibilizer POE-g-MAH were mixed uniformly, first kneaded at 160° C. for 2 minutes, and then transferred to a twin-screw extruder for extrusion granulation to obtain a wear-resistant and tear-resistant optical cable material;
[0059] Wherein, the preparation method of the modified boron nitride composite is as follows:
[0060] 15 g of hexagonal boron nitride and 3 g of nano-silicon dioxide were immersed in 150 mL of anhydrous ethanol, and then ball-milled after ultrasonic dispersion for 6 h. The ball-milled slurry was freeze-dried, ground, and sieved. It was sintered at 1600 ° C for 3 h, and the sintered body was placed in a diamond crushing and grading equipment for crushing and grading, and passed through a 400-mesh sieve to obtain a modified boron nitride composite.
[0061] The materials prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to performance tests, as follows:
[0062] Tensile strength and elongation at break: Tested in accordance with GB / T 2951 "General test methods for low-smoke and halogen-free electrical and optical cable and sheath materials";
[0063] Wear resistance: Each group of materials was tested on an Amsler wear tester, and the test parameters were: grinding disc: ψ122mm (ψ0.4ft), rotation speed: 185r / min, hardness: 58-60HRC, surface roughness: Ra=0.4um, grinding time: 2h, load: 30kg, and the wear rate, i.e., the mass loss rate, was tested;
[0064] The test results are shown in the following table:
[0065] Tensile strength(MPa) Elongation at break (%) Wear rate (%) Example 1 14.3 312 3.2 Example 2 14.9 331 2.1 Example 3 14.6 327 2.6 Example 4 14.5 318 2.7 Comparative Example 1 14.2 305 7.4 Comparative Example 2 12.4 196 3.9
[0066] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modifications or improvements made without departing from the spirit of the present invention are within the scope of the present invention.
Claims
1. A wear-resistant and tear-resistant optical cable material, characterized in that: The invention is prepared from the following raw materials by weight: 40-60 parts of low-density polyethylene, 5-10 parts of ethylene-vinyl acetate copolymer, 10-15 parts of modified boron nitride compound, 1-2 parts of calcium stearate, 3-5 parts of expandable graphite powder, 0.5-1 parts of zinc stannate, 0.4-0.8 parts of polyethylene wax, and 5-8 parts of compatibilizer; Wherein, the preparation method of the modified boron nitride composite is as follows: S1, immersing hexagonal boron nitride and nano-silicon dioxide in anhydrous ethanol, uniformly dispersing by ultrasonication, and then ball-milling, freeze-drying, grinding, sieving, high-temperature sintering, crushing and grading the ball-milled slurry, and then passing through a 400-mesh sieve to obtain a mixed powder; S2. Add stearic acid to anhydrous methanol solvent, heat and stir to dissolve, then add the mixed powder, continue stirring for 4-8 hours, filter the resulting suspension, wash and dry to obtain a modified boron nitride composite.
2. The wear-resistant and tear-resistant optical cable material according to claim 1, characterized in that: In step S1, the mass ratio of hexagonal boron nitride to nano-silicon dioxide is 10-15:2-3.
3. The wear-resistant and tear-resistant optical cable material according to claim 1, characterized in that: In step S1, the ball milling treatment time is 3-6 hours.
4. The wear-resistant and tear-resistant optical cable material according to claim 1, characterized in that: In step S1, the high temperature sintering temperature is 1400-1600°C, and the high temperature sintering time is 2-3h.
5. The wear-resistant and tear-resistant optical cable material according to claim 1, characterized in that: In step S2, the mass ratio of stearic acid, anhydrous methanol and mixed powder is 1-2:100:10-20.
6. The wear-resistant and tear-resistant optical cable material according to claim 1, characterized in that: In step S2, the temperature of heating and stirring is 55-65°C.
7. The wear-resistant and tear-resistant optical cable material according to claim 1, characterized in that: The compatibilizer is selected from POE-g-MAH or EVA-g-MAH.
8. The method for preparing the wear-resistant and tear-resistant optical cable material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: weighing low-density polyethylene, ethylene-vinyl acetate copolymer, modified boron nitride composite, calcium stearate, expandable graphite powder, zinc stannate, polyethylene wax and compatibilizer by weight, mixing all the raw materials evenly and kneading for 2-3 minutes, and then transferring them to a twin-screw extruder for extrusion granulation to obtain a wear-resistant and tear-resistant optical cable material.